Skip to content
Seeking US contractor partners IAS AC472 ACCREDITED ★ METAL BUILDINGS ★ AC472 IAS AC472 accreditedIAS AC472
World Steel USA
A steel member measured against its drawing dimensions at the World Steel plant

Engineering and codes

ASTM A6: the general rules behind every rolled shape and plate

A992, A572 and A36 are short documents because most of their rules live somewhere else: in ASTM A6. Mill tolerances, test frequency, marking, certificates and the list of extra tests an order can add all come from it. Here is how to use it.

· 7 min read · World Steel USA engineering team

Read ASTM A992 or A572 for the first time and they seem short. A few pages set chemistry and strength, and the rest says "see A6". ASTM A6 is where most of the rules live: how steel is ordered, tested, measured, marked and certified, what tolerances a rolled shape or plate may have, and which extra tests a purchaser can add. A reviewer who knows A6 can read any shape or plate certificate quickly and knows which questions to ask. This article is a practical guide to it.

The values below are a selection from current editions of ASTM A6/A6M and AISC 360-22. The editions named in the project specification govern.

What A6 covers

ASTM A6/A6M is the standard specification for general requirements for rolled structural steel bars, plates, shapes and sheet piling. It does not set strength or chemistry for any grade. Instead, each product specification, such as A36, A572, A588 or A992, says that the material shall conform to A6, and then adds its own grade requirements. Where the product specification and A6 disagree, the product specification governs.

AISC 360-22 Section A3.1 lists the product specifications that are approved for structural steel. All the rolled ones lean on A6.

Ordering information

A6 lists what an order should state, and a good material schedule follows it:

  • Quantity, by weight or number of pieces.
  • Name of the material: plate, W shape, angle, bar.
  • The product specification, grade and edition.
  • Dimensions, in metric or inch-pound units.
  • Condition, such as as-rolled, normalized or quenched and tempered, if the grade allows a choice.
  • Any supplementary requirement.
  • Any special requirement, such as a test report format.

When a mill receives an order without one of these, it supplies its normal practice. That is fine for ordinary material, and risky for anything special.

Chemical analysis

A6 requires a heat analysis for every heat: the chemistry of the steel as melted, taken from the ladle. That is the chemistry on the certificate. The purchaser may also ask for a product analysis, taken from the finished plate or shape, through supplementary requirement S2. Product analysis may differ slightly from heat analysis, and A6 gives the permitted variations.

The heat analysis is what welding engineers use to calculate a carbon equivalent and what galvanizers use to predict reactivity.

Tension testing

A6 sets how many tension tests are taken and where. For most as-rolled plate and shapes, tests are taken per heat and per thickness range or size group, with the location in the cross-section set by A6. For heat-treated plate, tests are taken per plate as heat-treated. The product specification then sets the yield, tensile and elongation the test must meet.

Two details are worth knowing:

  • Yield is measured by a stated method: the 0.2% offset or the extension-under-load method. The certificate should report the value, and the method if it matters.
  • Elongation depends on gauge length: 200 mm (8 in) or 50 mm (2 in). A certificate showing 21% must say which.

Mill tolerances

A6 has tables of permitted variations for every product. A few that matter on structural jobs:

Product What A6 limits
Plate Thickness, width, length, flatness, camber
W shapes Depth, flange width, flange tilt, web off-center, length, camber and sweep
Angles and channels Leg length, thickness, out-of-square, camber
Bars Size, out-of-round, straightness

Plate ordered by thickness may not be more than 0.3 mm (0.01 in) under the ordered thickness. Over-thickness is allowed within limits that grow with thickness and width.

For W shapes, camber and sweep are limited to about 1 mm per metre of length (1/8 in per 10 ft) for most sizes, with different rules for narrow flanges. That is why a long beam may arrive with some natural camber even if none was specified, and why cambering by the fabricator is a separate operation.

The AISC Code of Standard Practice uses these mill tolerances as the starting point. Fabrication tolerances apply on top of them, not instead of them. A dimension check at intake catches material outside A6 before it is cut.

Marking

A6 requires each piece, bundle or lift to be marked with:

  • The heat number.
  • The specification and grade, or a code for them.
  • The size.
  • The manufacturer's name, brand or trademark.

Marking may be by stencil, stamp, label or tag, as A6 allows for the product. In the fabricator's shop, the heat number must then be transferred to every cut part so that, after cutting, each piece can still be traced to its certificate. That transfer is a fabricator's quality practice, not an A6 rule, and it is one of the things IAS AC472 audits check.

Test reports and certification

A6 requires the manufacturer to report the results of the heat analysis and the mechanical tests, and any supplementary tests ordered. It also allows reports to be transmitted electronically. The EN 10204 system, which classifies certificates as 2.1, 2.2, 3.1 or 3.2, is the European way of saying who validated those results. A 3.1 certificate, validated by the mill's authorized inspection representative independent of production, is what we ask for on structural jobs. The EN 10204 mill certificate page explains the types.

A6 also allows material to be certified to more than one specification when it meets each one. Dual certification is common, and each specification claimed must be named on the report.

Supplementary requirements

The supplementary requirements are the part of A6 a designer uses most. They apply only when the order names them. The ones that come up on structural jobs include:

Requirement What it adds
S2 Product analysis Chemistry from the finished product, not just the heat
S5 Charpy V-notch impact test Toughness at a stated energy and temperature
S8 Ultrasonic examination Plate scanned for laminations and internal defects
S18 Maximum tensile strength An upper limit on tensile strength
S30 Charpy V-notch, alternate core location Toughness of heavy shapes taken where the steel cools slowest

S5 and S30 are the Charpy requirements AISC 360 and AISC 341 call on for heavy sections; see the Charpy V-notch article. S8 is often asked for on thick plate in T and corner joints where lamellar tearing is a concern. The ultrasonic testing page explains the method.

Each supplementary requirement needs its details stated: for S5, the energy, temperature, specimen orientation and test frequency (per heat or per piece); for S8, the acceptance standard.

Using A6 when reviewing a certificate

A practical review of a shape or plate certificate takes five steps:

  1. Confirm the product specification, grade and edition.
  2. Match the heat number to the steel and to the piece marks it will become.
  3. Check the chemistry against the product specification, using the heat analysis.
  4. Check yield, tensile and elongation, with the gauge length.
  5. Check every supplementary test the order named, and nothing missing.

The mill test certificate article walks through a real certificate.

Where A6 does not reach

A6 covers hot-rolled bars, plate, shapes and sheet piling. It does not cover hollow structural sections, pipe, sheet and strip, bolts or anchor rods. HSS have their tolerances in A500 and A1085, pipe in A53, sheet in A568 and A924 (through A1011 and A653), and fasteners in their own specifications. The rest of this series covers each.

Mill tolerance and fit-up in the shop

Mill tolerances become very real at fit-up. A W shape whose depth is at the plus end of its A6 tolerance meets a shear plate detailed for nominal depth; a flange slightly out of square leaves a gap under a stiffener; a plate at the plus end of its thickness changes the stack of a bolted joint. Good detailing allows for these variations with slotted holes, shims, finger fillers or field-adjustable details where they matter. Good shops measure critical dimensions on arrival, so a beam at the edge of its tolerance is fitted where it does no harm, or is set aside.

The AISC Code of Standard Practice also explains how mill tolerances combine with fabrication tolerances for columns, beams and assemblies, and the project specification may tighten them for architecturally exposed steel. Where a project has tight tolerances, for example a data hall floor, a crane runway or an exposed facade, the drawings should say so, so material can be selected and checked accordingly.

Common review questions on A6

  • "Does A6 require the certificate to be EN 10204 3.1?" No. A6 requires test reports with the specified results. The 3.1 type is a project or purchaser requirement that adds independent validation by the mill's inspection representative.
  • "Can a missing supplementary test be done later?" Often yes, on retained samples or on coupons cut from the material, at an accredited laboratory, if the engineer accepts it.
  • "Is a heat number on the bundle tag enough?" At intake, yes. Once pieces are cut, the number must be on each piece.

How World Steel uses A6 at intake

World Steel fabricates 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam. The steel comes mainly from leading Vietnamese mills, with Japan, Korea, Indonesia and Thailand when the project specification calls for them, and is ordered with the supplementary requirements your drawings name.

At our gate, every heat is matched to its EN 10204 3.1 certificate, marking is checked against A6, and shapes and plate are measured against the A6 tolerance tables before cutting. Heat numbers are transferred to every cut part and linked to piece marks in PEB Studio, and any check test runs at an ILAC-recognized ISO/IEC 17025 laboratory or the laboratory you name. Our incoming material checkpoint shows the steps, and all our grades are on the structural steel materials page. Next in the series: Charpy V-notch and heavy sections.

Quick answers

What does ASTM A6 cover?

The general requirements for rolled structural steel bars, plates, shapes and sheet piling: ordering information, chemical and tension testing, permitted variations in dimensions and mass, marking, test reports and a list of supplementary requirements a purchaser can add.

How thin can a plate be under ASTM A6?

Plate ordered by thickness may be no more than 0.3 mm (0.01 in) under the ordered thickness. Over-thickness limits depend on thickness and width and are given in the A6 tables.

What are A6 supplementary requirements?

Optional tests and limits that apply only when the order names them, such as product analysis (S2), Charpy V-notch impact testing (S5), ultrasonic examination of plate (S8), a maximum tensile strength (S18) and Charpy testing of heavy shapes at the alternate core location (S30).

Do fabrication tolerances replace mill tolerances?

No. Mill tolerances in ASTM A6 apply to the steel as rolled. Fabrication and erection tolerances in the AISC Code of Standard Practice and the project specification apply on top of them.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

ASTM steel grades series

Fifteen in-depth articles on the steel grades a US structural job names: what each ASTM specification covers, its strength and chemistry, where engineers use it, the extra requirements a project can add, and how a grade is sourced, checked and substituted.

Shapes and plate

The grades of the main frame: wide flanges, plate and the carbon steel of connections.

Hollow sections and pipe

Tube columns, braces and pipe, and the wall thickness the design may use.

Extra requirements

The general rules behind every grade, notch toughness and weathering steel.

Bolts, rods and sheet

The grades of what holds the frame together and the cold-formed steel around it.

Sourcing and substitutes

Grades rolled to other standards and how a substitution is asked for.

Bidding a large US project?

Send the bid documents, or just a footprint and an address. Our engineers check them against US code requirements and confirm what World Steel would supply, from a plant that fabricates 2,500 metric tons of structural steel a month.