Every bolted connection in a structural steel frame depends on a small part that is easy to overlook: the high-strength bolt. For decades, US structural bolts were ordered under two separate ASTM specifications, A325 and A490, with the twist-off bolts in two more. Since 2015 they have been grades of one standard, ASTM F3125. The names A325 and A490 survived as grade names, but the requirements were unified. This article explains the grades, their types and coatings, and the nuts and washers that must go with them.
The values below are a selection from current editions of ASTM F3125/F3125M and the RCSC Specification for Structural Joints Using High-Strength Bolts. The editions named in the project specification govern.
What F3125 covers
ASTM F3125/F3125M is the standard specification for high-strength structural bolts and assemblies, steel and alloy steel, heat treated, in inch and metric dimensions. It covers six grades:
| Grade | Head style | Minimum tensile strength |
|---|---|---|
| A325 | Heavy hex | 830 MPa (120 ksi) |
| A325M | Heavy hex, metric | 830 MPa |
| F1852 | Twist-off, round head | 830 MPa (120 ksi) |
| A490 | Heavy hex | 1,040 MPa (150 ksi), with a maximum |
| A490M | Heavy hex, metric | 1,040 MPa, with a maximum |
| F2280 | Twist-off, round head | 1,040 MPa (150 ksi), with a maximum |
One change from the old A325 matters: under F3125, A325 bolts have the same minimum tensile strength, 830 MPa (120 ksi), for all diameters. The old A325 had a lower value for diameters over 25 mm (1 in).
Inch bolts run from about 12.7 to 38.1 mm (1/2 to 1-1/2 in) in diameter; metric bolts from M12 to M36. US jobs normally use inch bolts, and the shop drawings should show the size the design used.
Types: plain and weathering
Each grade comes in Type 1, medium carbon or alloy steel, and Type 3, with weathering characteristics comparable to weathering steel such as A588. Type 3 bolts are used on bare weathering steel so the connection forms the same patina as the members. Type 3 is not a coating; it is the steel of the bolt.
Coatings: what each grade may take
Coating rules are where A325 and A490 differ most.
- A325 and F1852 may be hot-dip galvanized to ASTM F2329 or mechanically galvanized to ASTM B695 Class 55, and may take approved zinc-aluminum coatings. Galvanized A325 bolts are supplied with galvanized nuts, overtapped and lubricated, and the assembly is tested for rotational capacity.
- A490 and F2280 may not be hot-dip or mechanically galvanized. At their strength, the process risks hydrogen embrittlement, which can crack a bolt under load after installation. F3125 allows only specific coatings that have been shown not to cause it, such as zinc-aluminum to ASTM F1136 Grade 3.
That is why a galvanized frame almost always uses A325 bolts. Where a designer needs A490 strength on a galvanized structure, the coating must be one F3125 allows for A490, and that should be written on the drawings.
Nuts and washers
A bolt is one part of an assembly. The nut and washer must match its grade and coating.
| Bolt | Nut | Washer |
|---|---|---|
| A325, plain | ASTM A563 Grade C, DH, or A194 2H | ASTM F436 hardened |
| A325, galvanized | ASTM A563 Grade DH, galvanized, overtapped and lubricated | F436, galvanized |
| A490 | ASTM A563 Grade DH or A194 2H | F436 hardened |
| Type 3 weathering | Weathering nut grade | F436 Type 3 |
Galvanized assemblies should be supplied as a set by one manufacturer, because the nut overtapping and lubricant are matched to the bolt. Mixing a galvanized bolt from one source with a nut from another is a common cause of failed rotational capacity tests on site.
Joint types under RCSC
The RCSC Specification, which AISC 360-22 Section J3 adopts for high-strength bolting, recognizes three joint types:
- Snug-tight joints: plies in firm contact, bolts tightened by the full effort of a worker with a spud wrench or a few impacts. Common in gravity connections.
- Pretensioned joints: bolts tightened to a minimum pretension, for joints subject to load reversal, fatigue without slip concern, or where the design asks for it.
- Slip-critical joints: pretensioned bolts on faying surfaces with a qualified slip coefficient, for joints where slip would harm the structure, such as connections in fatigue or with oversized or slotted holes.
The joint type is the Engineer of Record's choice and is shown on the drawings. It affects the shop too: slip-critical faying surfaces must be left unpainted or coated with a qualified coating, which is masked or controlled during painting. The RCSC standard page covers the rules.
Pretensioning methods
RCSC allows four methods of reaching pretension: turn-of-nut, calibrated wrench, twist-off-type tension control bolts (F1852 and F2280) and direct tension indicators to ASTM F959. Each has its own pre-installation verification. Bolting and pretensioning on site are the US contractor's scope; the fabricator's part is to supply the right assemblies, keep them dry and lubricated, and keep each lot traceable.
A490: extra cautions
A490 bolts carry more load, which can reduce the number of bolts in a heavy connection. In return:
- They cannot be hot-dip or mechanically galvanized.
- They should not be reused after pretensioning.
- Welding to them, or heating them, is not allowed.
- They need care with hydrogen sources, including some cleaning and coating processes.
For most building frames, A325 is the default and A490 is used where its strength clearly pays off.
Marking and traceability
F3125 bolts are marked on the head with the grade, such as A325 or A490, the type where applicable, and the manufacturer's identification. Each production lot has a lot number, and test reports are issued per lot. On a structural job the bolt lot, nut lot and washer lot should all be traceable from the shipping list to the certificate, so the contractor's pre-installation verification uses the same assemblies that go into the frame.
Ordering structural bolts: what to write
- ASTM F3125/F3125M, the grade (A325, A490, F1852 or F2280) and the type (1 or 3).
- Diameter and length, with thread length suited to the grip.
- Coating: plain, hot-dip galvanized to F2329, mechanically galvanized to B695, or a zinc-aluminum coating, as allowed for the grade.
- Matching nuts (A563 grade) and F436 washers, with the same coating.
- Direct tension indicators to F959, if used.
- Lot test reports, and for galvanized A325, rotational capacity test results.
Bolts in galvanized and painted frames
Bolting is where coating systems and connection design meet.
- Galvanized frames normally use galvanized A325 assemblies. The faying surfaces of slip-critical joints in galvanized steel have a lower slip coefficient unless they are roughened or the coefficient is qualified, which the design must account for.
- Painted frames with slip-critical joints need either masked, unpainted faying surfaces or a coating tested and qualified for the slip class the design uses. The coating supplier provides the test data, and the shop drawings show the masked zones.
- Duplex systems, paint over galvanizing, combine both considerations and should be discussed before shop drawings are released.
Common review questions on bolts
- "Can we substitute A490 for A325?" Not automatically. A490 bolts are stronger, but they cannot be galvanized, should not be reused and may need different pretension and inspection.
- "The bolts arrived without nuts from the same supplier." For galvanized assemblies, that is a concern, because rotational capacity is tested per assembly lot. Ask for matched assemblies.
- "Are metric bolts acceptable on a US job?" Only if the design used them. Mixing inch and metric sizes is a common cause of field problems.
Storage and handling
High-strength bolts are sensitive to how they are stored. RCSC requires that fastener components be protected from dirt and moisture and that only as many as needed be taken from storage for a shift. Bolts that have rusted, lost their lubrication or been mixed between lots may not reach pretension correctly, and may fail the pre-installation verification. Galvanized assemblies are particularly sensitive to the lubricant on the nut.
For an overseas package, this means bolts should travel in sealed, labeled containers, kept separate from the steel, and be stored dry on arrival. Each container should show the grade, size, coating and lot numbers of the bolt, nut and washer, so the contractor's crew can match them to the certificate without opening every box.
Bolt length and thread in the grip
Bolt length is chosen so the thread does not run into the shear plane where the design assumes threads are excluded, and so there is enough thread for the nut and washers. RCSC gives the rules, and the bolt list on the shop drawings shows the length chosen for each connection. A length one size too short or too long can turn a correct grade into an incorrect connection.
How World Steel supplies bolts with the steel
World Steel fabricates 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam, and field bolts can be supplied with each package, listed by connection and piece mark on the bolt list. Bolts, nuts and washers are bought as matched assemblies to the F3125 grade and coating on your drawings, from suppliers in Vietnam or elsewhere in Asia as the grade and coating call for, and each lot travels with its test report, issued as an EN 10204 3.1 certificate when your specification asks for one.
Bolts are packed by lot, kept dry, and labeled so your crew can match each box to its certificate. Check tests, when your inspector wants them, run at an ILAC-recognized ISO/IEC 17025 laboratory or the laboratory you name. Our structural bolts page lists the assemblies, and the structural steel materials page lists every grade. Next in the series: F1554 anchor rods.
Quick answers
What is the difference between A325 and A490 bolts?
Strength. Under F3125, Grade A325 has a minimum tensile strength of 830 MPa (120 ksi) and Grade A490 has 1,040 MPa (150 ksi) minimum with an upper limit. A490 bolts carry more load but cannot be hot-dip galvanized and should not be reused once pretensioned.
What are F1852 and F2280 bolts?
Twist-off-type tension control bolts with a splined end that shears off when the bolt reaches pretension. F1852 has A325 strength and F2280 has A490 strength. Both are grades of ASTM F3125.
Can A490 bolts be galvanized?
Not by hot-dip or mechanical galvanizing, because of the risk of hydrogen embrittlement at their strength. F3125 allows only specific approved coatings, such as a zinc-aluminum coating to ASTM F1136 Grade 3, for A490.
Which nuts and washers go with F3125 bolts?
Heavy hex nuts to ASTM A563 (grade DH for galvanized A325 and for A490) or A194 Grade 2H, and hardened washers to ASTM F436, with coatings matched to the bolt.
Keep building your steel plan
Go further on USPEB.com
On this topic
Across the US market
- US codes and standardsIBC, AISC, AWS and MBMA, designed to
- Seismic steel structuresSDC D to F framing for West Coast jobs
- Crane building designUS crane standards for mill and bay buildings
- Design ReportWhat our US-code design report contains
- Large projects, 2,500 t a monthCapacity for large US general contractors
- Contractor partnershipLong-term supply for US contractors