Looking inside the weld
Sound goes into the weld, and anything that should not be there sends an echo back
A probe on the steel sends a short pulse of high-frequency sound into the joint at a known angle. Sound steel lets it pass; a crack, a lack of fusion or a slag line reflects part of it back. The instrument shows the echo as a peak on a screen, and its height and position tell the technician how big the reflector is and where it sits in the weld. That is why the US codes rely on UT for complete-joint-penetration welds: it sees the whole weld volume, from one side, with nothing to clear from the shop.
UT is the method AISC 360, AISC 341 and AWS D1.8 name for the welds that carry the frame.
Reading the screen
Four things on an A-scan, and how each is set
The screen is a time line. Everything the technician concludes comes from where an echo sits along it and how tall it stands against the reference.
The pulse leaving the probe, at the left of the screen.
A peak from a flaw. Its height, in decibels against the reference, rates the flaw.
The distance along the beam, which gives the flaw’s depth and position from the probe.
Set on a calibration block, so every echo is compared with the same known reflector.
Calibrated before the first weld
IIW-type reference block
Sets the sound path distance, the exit point and the real angle of each probe.
Reference sensitivity
A known hole in the block sets the reference level that every flaw echo is compared to.
Checks during the shift
Calibration is re-checked at set intervals and whenever the probe, cable or operator changes.
Couplant and surface
Clean, spatter-free scanning surfaces and couplant keep sound entering the steel consistently.
Beam angles
The angle follows the thickness
AWS D1.1 sets the angle to use by plate thickness and weld type. Probes around 2.25 MHz are the standard for structural welds; the procedure covers welds from 8 mm (5/16 in) to 200 mm (8 in) thick.
The usual first choice for the thinner range of groove welds, with a long, shallow path through the joint.
For mid-thickness welds and to confirm indications seen at 70°.
For thick welds and to scan the root of deep joints.
Straight beam: checks the plate itself for laminations before an angle-beam scan crosses it.
Accept or reject
Indication rating and the four severity classes
d = a − b − c
AWS D1.1 rates each indication as d = a − b − c: the gain to bring the echo to reference height (a), minus the reference level (b), minus an attenuation correction for the sound path (c). The rating, the weld thickness and the probe angle place the indication in one of four severity classes, with separate tables for statically and cyclically loaded connections.
Large discontinuities
Rejected whatever their length.
Medium discontinuities
Rejected above a short length limit.
Small discontinuities
Rejected above a longer length limit, or when too close to another indication.
Minor discontinuities
Accepted, regardless of length or location.
How much gets tested
Five sources of UT extent on a US job
We do not apply a fixed UT percentage of our own. These are the places the extent comes from, and the ITP shows which apply to your welds and who tests each.
All, or 10%, by risk category
CJP groove welds in butt, T- and corner joints under transverse tension, 8 mm (5/16 in) and thicker: all of them in Risk Category III or IV, 10% in Risk Category II. A quality assurance task for the owner’s agency.
CJP welds in the seismic system
UT of CJP groove welds 8 mm (5/16 in) and thicker in the seismic force-resisting system, plus base metal behind thick T- and corner joints checked for lamellar tearing.
Qualified procedure, tested technician
UT of demand-critical welds to a procedure qualified on mockups, by technicians who have passed the Annex F practical exam.
Crane runway girders
CJP flange-to-web welds 100% UT; flange and web splices 100% UT or RT.
Fabricator QC testing
Extra UT assigned to the fabricator by weld type and percentage. We perform what is assigned to us and record it in the ITP.
Straight beam
Testing the plate, not only the weld
Thick plate can carry laminations from the mill, and T-joints in thick plate can tear beneath the weld. A 0° beam finds both.
Laminations in plate
A straight-beam scan of plate, for example to ASTM A435 or A578, finds laminations before the plate is cut and welded.
Lamellar tearing
Thick plate pulled through its thickness at a T- or corner joint can tear below the weld. UT after welding looks for it.
Ordered with the steel
Where your specification calls for UT-tested plate, it is ordered and certified that way and the results come with the mill papers.
Who performs it
Who performs UT on your job
The Inspection and Test Plan both sides agree before production names who performs each test, where it happens and how the results come back to you.
In-house, by World Steel QC
Our QC performs UT to the extent your specification assigns to the fabricator, to written procedures, with calibrated equipment, at the plant in Vietnam.
Or by the third party you designate
Your QA agency, special inspector or testing firm can perform or witness UT at hold points in our plant, live by video alongside our QC, or on arrival at site.
Agreed in the ITP
Each UT line in the Inspection and Test Plan names the method, extent, acceptance criteria and who performs it, before production starts.
Weld types
The welds UT checks on your steel
Each weld type has its own landing: how it is sized, how we weld it, and how it is inspected.
The other methods
Five more ways we test a weld
Questions
Ultrasonic testing questions from US reviewers
Which welds are ultrasonically tested?
Those your specification and the governing code require. Typically CJP groove welds in butt, T- and corner joints, 8 mm (5/16 in) and thicker, in tension or in a seismic system, and crane girder welds under AIST TR-13. We do not apply a fixed percentage of our own.
Is code-minimum UT your job or our inspector’s?
AISC 360 Chapter N assigns its minimum UT to quality assurance, the owner’s agency. UT your specification assigns to the fabricator is performed by World Steel QC. Your agency can test at hold points in our plant, by video alongside our QC, or on arrival.
Who performs UT on our job?
World Steel QC in-house, or the third party you designate, or both: QC testing by us and QA testing by your agency on the same welds.
How are UT technicians qualified?
AWS D1.1 requires qualification to ASNT SNT-TC-1A, ANSI/ASNT CP-189 or ISO 9712. For demand-critical seismic welds, AWS D1.8 adds the Annex F hands-on exam. The technician’s qualification record is attached to each report.
Can UT be used on thin welds?
The AWS D1.1 UT procedure covers groove welds from 8 mm (5/16 in) to 200 mm (8 in). Thinner welds are inspected visually and, where needed, by MT or PT.
What happens if UT finds a flaw?
The indication is rated and, if rejectable, marked on the member, excavated and repaired under a qualified procedure, then tested again by UT. For seismic welds, AWS D1.8 Annex H flaw sizing may be used instead with the Engineer’s approval.
Is UT recorded so we can review it?
Conventional UT produces a written report per weld, with the indications, their ratings and locations. If you want the scan data itself saved for review, ask for phased array UT, which can be encoded and archived.
Send your weld map and UT requirements
We split every UT line into QC and QA in the ITP, plan the hold points with your agency, and file the results by piece mark.