US structural drawings name ASTM grades. Much of the steel rolled in Asia, and some of it in the US supply chain, is produced to other standards: JIS in Japan, KS in Korea, EN in Europe, and national standards elsewhere. Conversion tables on the internet line them up as steel grade equivalents: SS400 for A36, SM490 or S355 for A572 Grade 50. They are useful as a first guide, and misleading as a rule. This article shows where the common pairs differ, and how a US job should treat steel that was not rolled to the ASTM grade on the drawings.
The values below are selected from published editions of each standard for orientation only. The ASTM specification on the project governs, and any alternate is the Engineer of Record's decision.
Why it matters on a US job
AISC 360-22 Section A3.1 lists the ASTM specifications approved for structural steel. The International Building Code adopts AISC 360, so a US building official expects steel to meet those specifications. Section A3.1 also allows unidentified steel, free of injurious defects, only for members or details whose failure will not reduce the strength of the structure, locally or overall, and only with the Engineer of Record's approval. Everything else must be identifiable to an approved specification.
A grade from another standard is therefore not "equivalent" on a US job by default. It is either shown to meet the ASTM grade, accepted by the Engineer of Record as a substitution, or not used.
Common pairs and how they differ
| ASTM grade | Grade often called equivalent | Main differences |
|---|---|---|
| A36 | JIS G3101 SS400; KS D 3503 SS275; EN S275 | Yield values and how they fall with thickness; chemistry limits; SS400 has no carbon limit in the standard |
| A572 Grade 50 | JIS G3106 SM490; EN 10025-2 S355 | SM490 yield is lower than 345 MPa; S355 yield falls with thickness; EN sub-grades include Charpy |
| A992 | JIS G3136 SN490B or SN490C | SN490 has yield ratio and carbon equivalent limits like A992, but different values and thickness ranges |
| A500 Grade C | JIS G3466 STKR490; EN 10219 S355J2H | Wall tolerance, corner radius and strength basis all differ |
Yield that falls with thickness
The biggest trap is thickness. ASTM structural grades usually give one minimum yield for the full thickness range of the grade. JIS and EN usually step it down as thickness grows.
| Thickness | A572 Grade 50 | EN S355 | JIS SM490 |
|---|---|---|---|
| Up to 16 mm | 345 MPa | 355 MPa | 325 MPa |
| Over 16 to 40 mm | 345 MPa | 345 MPa | 315 MPa |
| Over 40 to 63 mm | 345 MPa | 335 MPa | 295 MPa |
| Over 63 to 80 mm | 345 MPa | 325 MPa | 295 MPa |
For thin plate S355 is slightly stronger than A572 Grade 50. For a 50 mm girder flange it is weaker. SM490 is below 345 MPa at every thickness; JIS SM490Y and SM520, with yields of about 365 MPa up to 16 mm, are the closer JIS matches in strength. A table that pairs grades by name hides all of this.
Chemistry and weldability
ASTM, JIS and EN limit chemistry differently. A992 caps carbon and carbon equivalent; A36 and A572 cap carbon by thickness; SS400 in JIS G3101 limits only phosphorus and sulfur, not carbon. A plate of SS400 can be perfectly good structural steel, but its weldability has to be judged from its actual chemistry on the certificate rather than from the standard. For welded members, the carbon equivalent from the heat analysis is the number to compare.
Toughness built into the grade name
EN 10025-2 includes Charpy toughness in its sub-grades:
- JR: 27 J at 20 °C.
- J0: 27 J at 0 °C.
- J2: 27 J at −20 °C.
- K2: 40 J at −20 °C.
An S355J2 plate therefore carries a toughness result that an A572 Grade 50 plate does not have unless the order adds Supplementary Requirement S5. That can make an EN grade attractive where the US design asks for Charpy testing, but the temperature and energy must still match what the drawings require. JIS SM490B and SM490C include Charpy at 0 °C; SM490A does not. The Charpy V-notch article explains how US requirements are written.
Section dimensions
Shapes are a second trap. A W shape is defined by the ASTM A6 dimension tables. JIS and EN H-sections and I-sections are rolled to their own dimension tables. Some come close to a W shape; few match it exactly in depth, flange width, thicknesses, root radius and mass. A design checked with W-shape properties cannot simply be built with a similar-looking H-section. For shapes, the only clean routes are a section rolled to the A6 table and certified to the ASTM grade, or a redesign with the actual section approved by the Engineer of Record.
SN steels: the closest idea to A992
Japan's JIS G3136 SN grades, steels for building structures, were developed for the same reasons as A992. SN490B and SN490C set an upper limit on yield, a maximum yield ratio and a carbon equivalent cap, and SN490C adds through-thickness requirements. In intent they are the nearest Asian match to A992 for seismic frames. In detail, the yield range, thickness steps and section sizes differ, so even SN steel goes through review before replacing A992.
Dual certification: the clean route
Many mills in Asia roll to ASTM specifications directly for export markets, or certify a product to both a national standard and an ASTM grade. A plate certified to an EN or JIS grade and also to A572 Grade 50, with test results meeting both, is A572 Grade 50 for a US job. Its certificate must name the ASTM specification and show the values ASTM requires. This is the route we prefer: the steel is bought to the ASTM grade from the start, and no substitution is needed.
When only another standard is available
Sometimes a size, thickness or delivery need points to steel rolled only to another standard. Then the steps are:
- Compare the certificate with the ASTM grade: chemistry, yield at the actual thickness, tensile, elongation, carbon equivalent and Charpy.
- Where values are missing or not tested the ASTM way, run supplementary tests at an accredited laboratory.
- Submit the comparison to the Engineer of Record as a substitution request, with the effect on design shown.
- Proceed only with written acceptance, and keep the record with the heat.
The grade substitution article describes the request in detail.
What not to do
- Do not accept a material because a conversion table says it is equivalent.
- Do not relabel steel. The certificate and the marking must show what the steel was rolled and tested to.
- Do not mix similar grades of different standards on one member without the engineer's knowledge.
A worked example: S355 plate for an A572 Grade 50 girder
Suppose a girder is designed with A572 Grade 50 plate: a 50 mm flange and a 16 mm web. A mill offers S355J2 plate. The comparison would note:
- Web, 16 mm: S355 yield 355 MPa, above A572 Grade 50's 345 MPa. Acceptable on strength.
- Flange, 50 mm: S355 yield 335 MPa for 40 to 63 mm, below 345 MPa. Not acceptable unless the actual test result is 345 MPa or more and the engineer accepts the tested value, or the design is checked with 335 MPa.
- Toughness: J2 gives 27 J at −20 °C, which may meet or exceed a project Charpy requirement; the temperature must be compared with the drawings.
- Chemistry: S355J2 limits carbon and carbon equivalent; the heat analysis is compared with the welding procedure.
The answer is not "equivalent" or "not equivalent". It is a set of facts for the engineer, and often a dual-certified plate is the simpler choice.
Certificates in other languages and formats
Certificates from Asian mills are often bilingual, with the national standard's terms beside the English. EN 10204 certificate types are widely used, which helps, because a 3.1 certificate means the same thing whichever country it comes from. A reviewer should still confirm three things: that the ASTM specification and grade are named, that the units are clear (MPa or N/mm² are the same; ksi values may be converted), and that the test methods are those ASTM requires, or that the engineer accepts the method used.
When in doubt, a check test at an accredited laboratory settles the question for that heat. ILAC recognition means a laboratory accredited in one member country is recognized by accreditation bodies in the others, so a test report from an ISO/IEC 17025 laboratory in Vietnam carries the same standing as one from a US laboratory under the same scope.
How World Steel handles steel from other standards
World Steel fabricates 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam. The steel comes mainly from leading Vietnamese mills, including Hoa Phat, Formosa Ha Tinh and POSCO among our sources, with Japan, Korea, Indonesia and Thailand when the project specification calls for them. Steel is ordered to the ASTM specification and grade on your drawings; where a mill works to another standard, the comparison goes to your Engineer of Record before anything is ordered.
Every heat is matched to its EN 10204 3.1 certificate at our gate, and any supplementary test runs at an ILAC-recognized ISO/IEC 17025 laboratory or the laboratory you name. Mill names are sourcing only; the mill on each certificate is the record. All the grades we supply are on the structural steel materials page. Last in the series: steel grade substitutions.
Quick answers
Is SS400 the same as A36?
No. They are close, but SS400 has a lower minimum yield for most thicknesses, 245 MPa against 250 MPa for A36 up to 16 mm, falling further as thickness grows, and its chemistry limits differ. It can be accepted only if the Engineer of Record agrees after comparing the certificate with A36.
Is S355 equivalent to A572 Grade 50?
Close in strength for thin plate, but S355 yield falls with thickness, to 345 MPa from 16 to 40 mm and lower beyond, while A572 Grade 50 keeps 345 MPa (50 ksi) up to 100 mm (4 in). EN sub-grades such as J2 add Charpy requirements that A572 does not have by default.
Which Asian grade is closest to A992?
JIS G3136 SN490B or SN490C, steels for building structures with an upper yield limit, a yield ratio limit and a carbon equivalent cap, the same ideas behind A992. Their values and section dimensions still differ from A992 and the A6 tables.
Can steel rolled to another standard be used on a US job?
Only with the Engineer of Record's acceptance, and where required the building official's. AISC 360 Section A3.1 lists ASTM specifications; other steel is a substitution that must be shown to meet the specified grade.
Keep building your steel plan
Go further on USPEB.com
On this topic
Across the US market
- US codes and standardsIBC, AISC, AWS and MBMA, designed to
- Seismic steel structuresSDC D to F framing for West Coast jobs
- Crane building designUS crane standards for mill and bay buildings
- Design ReportWhat our US-code design report contains
- Contractor partnershipLong-term supply for US contractors
- Solutions by stateState-by-state steel solutions