Skip to content
Seeking US contractor partners IAS AC472 ACCREDITED ★ METAL BUILDINGS ★ AC472 IAS AC472 accreditedIAS AC472
World Steel USA
Galvanized ladder cage ready for coating thickness checks at World Steel

Coatings and durability

Measuring galvanized coating thickness: the four ASTM A123 methods

ASTM A123 allows four ways of measuring galvanized coating thickness. On structural steel one of them does almost all the work, but knowing the other three, and the referee method for disputes, saves arguments at acceptance.

· 7 min read · World Steel USA engineering team

Every galvanized lot is accepted or rejected on numbers, and the numbers depend on how they were taken. ASTM A123 allows four methods for measuring galvanized coating thickness, and a fifth procedure, the referee method, for settling disputes. On structural steel the magnetic gauge does almost all the work, but each method has its place. This article explains them, with the practical points that decide whether a reading means anything.

The edition reviewed is ASTM A123/A123M-13. The test methods it refers to, ASTM E376, A90 and B487, are separate standards, and the editions your specification names govern.

Where to measure: the specimen

Before any method, the inspector must know what is being measured. Section 3.2.9 defines a specimen as the surface of an article, or of a portion of it, on which measurements are taken. A piece with a surface area of more than 100,000 mm² (160 sq in) is split into three specimens of about equal area; a smaller piece is one specimen. Each material category and steel thickness on the piece is its own specimen.

For magnetic measurements, Section 3.2.9 also excludes surfaces that have been flame cut, machined or threaded, or that the method cannot read reliably, because they do not represent the general surface. Section 3.2.10 then defines the specimen coating thickness as the average of at least five readings, placed so that they spread as widely as possible across the specimen.

That is the frame for everything below: five or more spread readings, averaged, per specimen.

Method 1: magnetic gauges (Section 8.2.1)

Section 8.2.1 makes magnetic thickness measurement to ASTM E376 the default, unless one of the other methods is used. For each specimen, five or more readings are taken at points widely dispersed through the volume the specimen occupies, so they represent as much of its surface as practical. Their average is the specimen coating thickness.

The rest of Section 8.2.1 sets out how the averages roll up:

  • Multi-specimen articles (8.2.1.1). The average of the three specimen grades is the average coating thickness of the test article. A specimen is evaluated for each steel category and thickness within each specimen of the article.
  • Single-specimen articles (8.2.1.2). The average of all the specimen grades is the average coating thickness for the sample.
  • Threaded parts (8.2.1.3). Readings are taken on a part of the article without threads.
  • Where gauges fit (8.2.1.4). Magnetic methods suit large articles, and small ones when there is enough flat surface for the probe tip to sit flat.

Gauge types

Two kinds of gauge are in common use:

  • Magnetic pull-off gauges measure the force needed to pull a magnet off the surface, which falls as the coating gets thicker. They are simple and need no batteries, but are slower and more sensitive to how they are held.
  • Electronic gauges using magnetic induction, such as the Elcometer 456 used under World Steel's galvanizing procedure, read the coating directly, store readings and calculate averages. They are the norm on structural work.

Getting readings that mean something

A gauge is only as good as its setup. Good practice, in line with E376 and the gauge maker's instructions:

  • Verify the gauge on certified reference standards or shims before use and at intervals during the shift, in the thickness range being measured.
  • Zero on bare steel of similar thickness and curvature where the gauge type needs it.
  • Keep away from edges and corners, where the magnetic field is distorted; the gauge maker states the minimum distance.
  • Watch thin steel and curved surfaces, both of which affect readings.
  • Clean the surface of loose zinc ash or flux that would lift the probe.
  • Record each reading by specimen, not only the averages, so the arithmetic can be checked.

Method 2: stripping (Section 8.2.2)

The stripping method follows ASTM A90. A test article, a specimen cut from one, or a group of very small items such as nails is weighed, the zinc is dissolved in an acid solution that does not attack the steel, and the piece is weighed again. The loss of weight per unit area is the coating weight, converted to thickness with Table 2.

Section 8.2.2.1 says stripping is destructive and suits single-specimen articles, but is not practical for multi-specimen articles. In practice it is used on fasteners, small castings and small brackets.

Method 3: weighing before and after (Section 8.2.3)

Here the article is weighed after pickling and drying, before galvanizing, and again after it has cooled to room temperature. The difference divided by the surface area is the coating weight, again converted with Table 2. Section 8.2.3.1 limits it to single-specimen articles.

The 10 % caution

Note 11 applies to both stripping and weighing. Neither method accounts for the iron from the article that is incorporated into the zinc-iron alloy layers, so both can underestimate the coating weight, and the thickness calculated from it, by up to 10 %. Their accuracy also depends on how accurately the surface area of the articles is known, which is hard on complex shapes.

Method 4: microscopy (Section 8.2.4)

The microscopy method follows ASTM B487. A cross-section is cut through the coating, mounted, polished and measured under an optical microscope. Each measurement is a point value, and at least five are taken at locations spread as widely as practical over the article. Their average is the specimen coating thickness.

Section 8.2.4.1 calls it a destructive test suited to single-specimen articles and impractical for multi-specimen articles. It is also the only method that shows the individual zinc-iron alloy layers, so it is useful for investigating unusual coatings.

Which method fits which piece

Method Destructive Best for Section
Magnetic gauge, ASTM E376 No Structural members, plate, tubing, assemblies 8.2.1
Stripping, ASTM A90 Yes Fasteners and small parts 8.2.2
Weighing before and after No, but needs the black weight Small single-specimen parts 8.2.3
Microscopy, ASTM B487 Yes Small parts, investigations 8.2.4

The referee method (Section 8.2.5)

When the purchaser and galvanizer disagree on coating thickness, Section 8.2.5 sets out how the dispute is resolved.

For multi-specimen articles (8.2.5.1), a new sample is taken at random from the lot, with twice as many test articles as the sample that failed. If the lot is too small to double the sample, the sample stays the same size but the number of widely dispersed measurement sites is doubled, and those sites form the new sample. The new sample is measured with magnetic gauges calibrated for accuracy against reference thickness standards.

For single-specimen articles (8.2.5.2), a new random sample twice the size of the failed one is taken, and the test method is chosen by agreement between purchaser and galvanizer.

If the new sample still shows the lot to be nonconforming, the galvanizer has the right to sort the lot by testing each article, to regalvanize the nonconforming articles, or to repair them under Section 6.2.

Common measurement mistakes

Most thickness disputes come from one of these:

  1. Treating a whole large member as one specimen instead of three.
  2. Measuring flame-cut edges, threads or machined faces.
  3. Rejecting on one low reading instead of the specimen average, contrary to Section 6.1.3.
  4. Applying the wrong Table 1 line, for example the shapes line to plate.
  5. Using a gauge that was not verified in the right thickness range.
  6. Reading on loose zinc ash or a wet surface.

The lot and sampling side of acceptance is covered in lots and sampling under ASTM A123, and the grades themselves in ASTM A123 coating thickness grades.

Reading thin and curved steel

Two situations need extra care with magnetic gauges. On thin steel, the magnetic field can pass through the steel and the reading drifts; the gauge maker states a minimum steel thickness, and readings on thinner parts are checked against a reference on steel of the same thickness. On curved surfaces such as small pipe and round bar, the probe may rock; a probe designed for curved surfaces, or a zero set on bare steel of the same curvature, keeps the readings honest. Where neither works, the small part is better measured by one of the weight methods, which is exactly what Section 8.2.1.4 suggests.

How many readings is enough

Five readings per specimen is the minimum the standard sets, not a target. On a long member, five readings spread over each third gives fifteen readings for the article. Inspectors often take more on large or complex pieces, and nothing in the standard prevents it, as long as the readings stay widely dispersed rather than clustered in one spot. More readings make the average more reliable and reduce the chance that one unusual area decides the result.

How World Steel measures and records the zinc

World Steel fabricates up to 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam. Galvanizing is arranged in Vietnam with a galvanizer named for the job, under our written galvanizing procedure, and coating thickness is read on every lot with an Elcometer 456 magnetic-induction gauge, verified on reference standards. Readings are recorded per specimen with the material category and steel thickness, averaged as A123 requires, and filed on a thickness inspection sheet by piece mark.

Your inspector, or a third-party agency you appoint, can witness the readings at the galvanizer in person or follow them live by video, and the sheets are posted in PEB Studio. See how we organize inspection on our coating inspection page, and the standard at a glance on our ASTM A123 page.

Quick answers

How is galvanized coating thickness measured on structural steel?

With a magnetic thickness gauge used to ASTM E376, taking at least five readings spread widely over each specimen. It is the default method in ASTM A123 Section 8.2.1 and is non-destructive.

When are stripping or weighing used?

For small single-specimen articles such as fasteners or small brackets, where a gauge probe cannot sit flat. Both methods are destructive or need the piece weighed before galvanizing, and they are not practical for large multi-specimen articles.

Why can weighing underestimate the coating?

Note 11 explains that stripping and weighing do not count the iron from the steel that becomes part of the alloy layers, so they can underestimate coating weight, and the calculated thickness, by up to 10 %.

What happens if the buyer and galvanizer disagree on thickness?

Section 8.2.5 sets a referee method: a new random sample twice the size of the failed one, measured with calibrated magnetic gauges for large articles, or by an agreed method for small ones. If the lot still fails, the galvanizer may sort, regalvanize or repair.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

ASTM A123 hot-dip galvanizing series

Sixteen in-depth articles that follow a galvanized member from the coating specification, through design for the kettle and the dip itself, to the thickness gauge, the repair rules and the jobsite. Each one explains a part of ASTM A123 in plain terms and lists what to check.

Specify and order

What A123 covers, what goes on the order, and the steel and zinc chemistry behind the coating.

Design for the kettle

Vent and drain holes, distortion, embrittlement and welded assemblies.

Through the kettle

The hot-dip process step by step and the zinc-iron layers it grows.

Thickness and sampling

Coating grades by steel, how the zinc is measured and how a lot is sampled.

Finish, repair and the site

What the finish may show, A780 repairs, inspection and retest, and storage on the way to the job.

Bidding a large US project?

Send the bid documents, or just a footprint and an address. Our engineers check them against US code requirements and confirm what World Steel would supply, from a plant that fabricates 2,500 metric tons of structural steel a month.