Paint sits on top of steel. A hot-dip galvanized coating grows out of it. When a fabricated member is lowered into molten zinc, the zinc reacts with the iron at the surface and forms a stack of zinc-iron alloy layers, topped by a layer of nearly pure zinc as the member is withdrawn. That structure is what makes galvanizing different from every other coating on a steel job, and it explains much of what ASTM A123 says about finish, appearance and adherence. This article looks inside the coating.
The layer values given here are typical industry figures, not requirements of ASTM A123. The standard sets minimum coating thickness and finish; it does not specify the layers. The edition reviewed is A123/A123M-13.
The four layers, from the steel out
A polished cross-section of a typical coating on structural steel shows four layers:
| Layer | Approximate zinc content | Character |
|---|---|---|
| Gamma | about 75 % zinc | Very thin, next to the steel, tightly bonded |
| Delta | about 90 % zinc | Dense, compact alloy |
| Zeta | about 94 % zinc | Columnar crystals, often the thickest alloy layer |
| Eta | about 100 % zinc | Soft outer zinc, frozen from the bath on withdrawal |
The gamma, delta and zeta layers are intermetallic compounds: fixed ratios of zinc and iron with their own crystal structure. They grow by diffusion while the steel is in the bath. The eta layer is simply bath metal that solidifies on the surface as the member comes out.
Our ASTM A123 page draws the four layers next to the coating grade finder.
How the layers grow in the kettle
When clean, fluxed steel enters zinc at about 450 °C (842 °F), the flux burns off and zinc meets bare iron. Iron dissolves into the zinc at the surface, and the alloy layers begin to form almost at once. They keep growing as long as the steel is in the bath, quickly at first and then more slowly, because each layer acts as a barrier that zinc and iron must diffuse through.
The galvanizer controls three things that affect growth:
- Bath temperature. Higher temperatures generally speed growth.
- Immersion time. Longer dips grow thicker alloy layers. A heavy section also takes longer to reach bath temperature, so it stays in longer.
- Bath chemistry. Section 5.5 of A123 requires at least 98.0 % zinc in the working bath, and Note 3 allows trace additions of aluminum, nickel and tin. Nickel in particular slows the reaction on some reactive steels.
The steel controls the rest. Note 2 explains that silicon, carbon and phosphorus in the steel or weld metal can speed up alloy growth so much that the alloy reaches the surface, leaving a matte finish with little or no outer zinc. The details are in reactive steel and the zinc bath.
Why the coating is so hard to knock off
Two properties of the alloy layers matter on a construction job.
Hardness. The zeta and delta layers are harder than mild structural steel. Typical hardness figures published by the galvanizing industry put them well above the steel underneath, with the outer eta layer softer. In practice the hard alloy resists abrasion from slings, chains and dunnage, and the soft eta layer absorbs light impacts. That is why galvanized steel survives an ocean voyage and erection better than most paint systems.
Bond. Because the alloy layers grow out of the steel, the coating is bonded metallurgically. Paint bonds by adhesion and can be measured in a pull-off test in megapascals; galvanizing is part of the metal. Section 6.5 of A123 sets the expectation: the zinc coating must withstand handling consistent with its nature and thickness and the normal use of the article, without peeling or flaking.
The limits of the alloy
Hard alloy is also less ductile than pure zinc. Note 9 of A123 states that the coating is generally too heavy to allow severe bending without damage, even though some material may be formed after galvanizing. Severe bends can crack the alloy layers and flake the coating.
Thick coatings on reactive steel, where the alloy makes up most of the thickness, are the most brittle. They protect just as well, but they can chip at sharp edges if a member is dropped or struck. Handling rules on site follow from that: nylon slings, padded supports and no dragging on edges.
Bright, spangled and gray finishes
The look of a new galvanized coating comes from its top layer.
- Bright and spangled. When a full eta layer freezes on the surface, the zinc forms crystals that can show as a spangle pattern. It is common on low-silicon steel.
- Bright but even. Bath additions and cooling change the crystal size; many modern coatings are bright with little visible spangle.
- Matte gray. When the alloy layers grow right through to the surface, there is little or no eta zinc, and the coating looks dull gray, sometimes in patches.
- Mixed. A member made of different steels can show bright and gray areas side by side.
ASTM A123 Section 6.2 is clear that minor roughness and appearance related to steel chemistry or reactivity are not grounds for rejection. A gray coating is not a defect, and it usually carries more zinc. Over time all galvanized coatings weather to the same dull gray as the zinc forms its patina.
The patina: how zinc protects over time
Freshly galvanized zinc is reactive. Exposed to air, it forms zinc oxide, then zinc hydroxide in the presence of moisture, and finally, with carbon dioxide in the air, a stable zinc carbonate film. That patina is what slows corrosion of the zinc in normal outdoor exposure. It needs air and cycles of wetting and drying to form, which is why new galvanized steel stacked tightly and kept wet can develop white powdery wet storage stain instead.
Under the patina, the zinc protects the steel in two ways. It is a barrier between the steel and the environment, and it is sacrificial: where the coating is scratched, the zinc around the scratch corrodes first and protects the bare steel. That sacrificial action is also why small repaired areas, covered in repairing galvanized coatings, work when they are kept within the limits of Section 6.2.
Dross and inclusions
The bath also produces a by-product: dross, small particles of zinc-iron alloy that form as iron dissolves into the zinc and settle at the bottom of the kettle. Finely dispersed dross particles in the coating show as small pimples and are harmless. Section 3.2.4 of A123 defines gross dross inclusions as zinc-iron intermetallics present in a form other than finely dispersed pimples: raised lumps that would leave a bare spot if knocked off. Section 6.4 requires galvanized articles to be free of them when they leave the galvanizer.
Dross control is part of bath management: skimming the surface before withdrawal, removing dross from the bottom of the kettle, and keeping the flux and rinse baths clean so less iron reaches the zinc.
What the layers mean for duplex systems
When galvanized steel is painted, the paint bonds to the outer zinc or alloy surface. Fresh zinc is smooth and reactive, so it needs preparation: a light sweep blast to SSPC-SP 16 or another method the paint manufacturer accepts. Steel for painting is cooled in water or air instead of a chromate passivation, because the passivation film stops paint bonding. Our SSPC page covers the preparation, and duplex coating systems covers the products.
Checking the coating without cutting it
The layers are only visible under a microscope on a polished cross-section, which is the method of ASTM B487 named in Section 8.2.4 of A123. It is destructive and is used for small parts or disputes. On structural members the total coating thickness is read with a magnetic gauge to ASTM E376, which measures all the layers together. The next articles in this series cover coating thickness grades and how the zinc is measured.
What the layers mean for handling and erection
The structure of the coating suggests a few handling rules on site. The hard alloy resists scuffing from slings and dunnage, so galvanized members tolerate rough handling better than painted ones. The soft outer zinc can still be marked, and a thick, mostly alloy coating on reactive steel can chip at sharp edges if a member is dropped. Nylon slings, padded supports, lifting rather than dragging, and keeping chains off edges protect both. Any area knocked down to bare steel is repaired with an ASTM A780 method, and the zinc around it protects the steel while the repair is made, which is one of the reasons small damage does not spread rust under galvanizing the way it can under paint.
Why the layers matter for bolted connections
Galvanized faying surfaces in slip-critical joints are a special case. The outer zinc is soft and slippery, so as-galvanized surfaces have a low slip coefficient unless they are roughened, for example by a light blast or wire brushing done as the RCSC Specification allows for the slip class used. Snug-tight and pretensioned bearing joints do not depend on friction and need no treatment. The joint type is set by the Engineer of Record, and the surface treatment goes on the shop drawings.
How World Steel uses this on US jobs
World Steel fabricates up to 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam. On galvanized jobs, the coating is arranged in Vietnam with a galvanizer named for the job, under our written galvanizing procedure: zinc of 99.99 % purity, a bath at 440 to 450 °C (824 to 842 °F) sampled monthly by TÜV Rheinland, and an immersion of three to five minutes by steel thickness.
Because the chemistry of every heat of steel is on file, we can tell an owner before fabrication which members are likely to come out matte gray, so the appearance is agreed rather than argued at delivery. Coating thickness is read on every lot and the records travel with the steel in PEB Studio. See the procedure on our hot-dip galvanizing page.
Quick answers
What are the layers of a hot-dip galvanized coating?
From the steel outward: a thin gamma layer of about 75 % zinc, a delta layer of about 90 % zinc, a zeta layer of about 94 % zinc and an outer eta layer of pure zinc. The first three are zinc-iron alloys grown by reaction with the steel.
Why are the alloy layers harder than the steel?
Zinc-iron intermetallic compounds are hard by nature. Typical hardness values for the zeta and delta layers are higher than for mild structural steel, which is why galvanizing resists abrasion and knocks in transit.
How is a galvanized coating bonded to the steel?
Metallurgically. The alloy layers grow out of the steel surface by diffusion, so the bond is part of the metal rather than a paint-like adhesive layer. ASTM A123 Section 6.5 requires the coating to withstand normal handling without peeling or flaking.
Does a gray coating without the outer zinc protect as well?
Yes. Protection depends on the mass of zinc, and gray coatings from reactive steel are usually thicker. ASTM A123 does not allow rejection for roughness or color caused by steel chemistry.
Keep building your steel plan
Go further on USPEB.com
On this topic
Across the US market
- Steel fire protectionIntumescent and fire-rated steel packages
- Quality hubCoating inspection by FROSIO Level III inspectors
- Products catalogGalvanized, painted and built-up members
- Download centerSample ITP, design report and approval drawings
- Large projects, 2,500 t a monthCapacity for large US general contractors
- Contractor partnershipLong-term supply for US contractors