Repairing galvanized coatings: A123 limits and the three ASTM A780 methods

Small bare spots on galvanized steel are repaired, not rejected, as long as they stay within limits. Repairing galvanized coatings has two rulebooks: ASTM A123 says how much may be repaired, and ASTM A780 says how. Here are both, with a worked example.

· 7 min read · World Steel USA engineering team

No galvanizing line produces a perfect coating every time. A hanging point leaves a small bare mark, a weld spatter pops off, a member is scraped as it is lifted out. ASTM A123 accepts that and allows small areas to be repaired, which it calls renovation, rather than sending every piece back through the kettle. Repairing galvanized coatings is governed by two documents: A123 sets how much may be repaired and how thick the repair must be, and ASTM A780 sets the repair methods. This article covers both.

The editions reviewed are ASTM A123/A123M-13 and the A780 practice it refers to. The editions your specification names govern.

Who repairs, and when

Section 6.2 says surfaces that remain uncoated after galvanizing shall be renovated using the methods of ASTM A780, unless the purchaser directs the galvanizer to leave them untreated for later renovation by the purchaser. By default, then, the galvanizer repairs before shipment.

Repairs needed later, because of damage in transport, at erection or from site welding, are outside the galvanizer's A123 scope and follow the project specification, usually with the same A780 methods.

The size limits

Three limits decide whether a bare area may be repaired.

Each area. Section 6.2.1 says each area subject to renovation must be 25 mm (1 in) or less in its narrowest dimension. A long narrow scratch can qualify; a wide patch cannot.

Total per article. Section 6.2.2 says the total area subject to renovation on each article must be no more than 0.5 % of the accessible surface area to be coated on that article, or 256 cm² per metric ton of piece weight (36 sq in per short ton), whichever is less.

Accessibility. Section 6.2.4 says that when the areas needing renovation exceed those criteria, or are inaccessible for repair, the coating is rejected. Note 5 defines inaccessible surfaces as those that cannot be reached for proper surface preparation and application of repair materials under A780, giving the inside of certain tanks, poles, pipes and tubes as examples.

A rejected piece is not lost. Section 9.6 allows material rejected for reasons other than embrittlement to be stripped, regalvanized and submitted again.

A worked example

Take a welded built-up girder weighing 2 metric tons with a coated surface of about 30 m² (about 320 sq ft).

  • 0.5 % of 30 m² is 0.15 m², which is 1,500 cm².
  • 256 cm² per metric ton times 2 tons is 512 cm².
  • The smaller value governs, so at most 512 cm² of the girder may be repaired, in areas no wider than 25 mm (1 in) each.

For light members the weight rule usually governs, because they have a lot of surface for their weight. For very heavy, compact members the percentage rule can govern.

World Steel's tighter limits

World Steel's written galvanizing procedure sets limits that are tighter than A123 for steel galvanized for our jobs: no more than 0.5 % of the surface and no more than 250 cm² (about 39 sq in) in total per piece, with no single spot larger than 40 cm² (about 6 sq in). Anything beyond those limits, or outside A123, goes back through the acid and the kettle. Repairs are made with zinc-rich coating to ASTM A780.

The three A780 methods

ASTM A780 describes three ways of renovating a galvanized coating. Each has its own surface preparation and application rules, and the material supplier's instructions apply alongside the practice.

Zinc-based solder

A zinc alloy solder, in stick or powder form, is melted onto the cleaned and preheated area, usually with a torch. The preparation is wire brushing, light grinding or a light blast to clean metal, and the surrounding coating is heated carefully so as not to burn it. Solder gives a metallic repair closest to the original zinc, but the heating makes it slower and less suited to large or vertical areas.

Zinc-rich paint

A paint with a high content of zinc dust in the dry film is brushed or sprayed onto the cleaned area. A780 sets the zinc content the paint must contain and refers to SSPC cleaning grades for preparation, typically power-tool or blast cleaning to bright metal, overlapping onto sound galvanizing. Zinc-rich paint is the most common method, because it is simple, portable and suits field work.

Sprayed zinc (metallizing)

Zinc wire or powder is melted and sprayed onto an abrasive-blasted surface with a thermal spray gun. The repair is metallic and can be built to thickness quickly over larger areas, but it needs blasting equipment and a trained operator.

Method Preparation Strengths Limits
Zinc-based solder Clean to bright metal, preheat Metallic, close to original zinc Heat, slow, small areas
Zinc-rich paint Power tool or blast to bright metal Simple, portable, common Needs extra thickness
Metallizing Abrasive blast Metallic, fast on larger areas Equipment and skill

How thick the repair must be

Section 6.2.3 says the thickness of renovation must be the thickness grade required by Table 1 for the material category and steel thickness, measured as Section 6.1 describes. There is one exception: for renovation with zinc paints, the thickness must be 50 % higher than Table 1, but not greater than 100 µm (4.0 mils).

So a repair on a structural shape 10 mm thick, where Table 1 asks for 100 µm (3.9 mils), needs 100 µm of solder or metallized zinc, or 100 µm of zinc-rich paint, because 50 % more than 100 µm would exceed the 100 µm (4.0 mils) cap. A repair on 5 mm plate, where Table 1 asks for 75 µm (3.0 mils), needs 75 µm of metallic repair or about 100 µm (4.0 mils) of zinc-rich paint, again at the cap. Repairs are measured with the same magnetic gauge as the coating.

Handling marks and contact points

Section 6.4 says marks from tongs and other handling tools are not a cause for rejection unless they have exposed the base metal and the bare areas exceed the limits of Sections 6.2.1 and 6.2.2. In practice hanging-wire and hook marks are small, bare and within the limits, and are repaired before release.

Repairs on site

After delivery, damage from slings, transport, bolting up or site welding is repaired by the US contractor, our customer, as part of the site work. Good practice:

  1. Clean the damaged area and a margin of sound zinc around it to bright metal.
  2. Apply an A780 method, usually zinc-rich paint, to the thickness required.
  3. Measure the repair with a magnetic gauge.
  4. Record the location, size, method and product.

Field welding of galvanized steel needs the zinc removed from the weld zone first, with ventilation for zinc fumes, and a repair afterwards. Bolted field connections avoid it.

Our coating submittals list the repair product and procedure, and the brands we use for zinc-rich products are sold through their own US distributors, so the same product can be bought near the job.

Recording repairs

A repair record turns a judgment call into evidence. For each repaired piece it should give the piece mark, the location and size of each area, the method and product, and the measured thickness. The record shows the reviewer that the area was within the Section 6.2 limits and that the repair reached the Section 6.2.3 thickness.

When to redip instead of repair

Repair is the right answer for small, accessible defects. Redipping is the better answer when:

  • the bare area is wider than 25 mm (1 in) in its narrowest dimension,
  • the total area to repair is over the Section 6.2.2 limit,
  • the defect is inside a hollow section or another surface that cannot be reached,
  • the coating thickness is below the grade over a large area,
  • the piece is critical to appearance and a visible repair is not acceptable.

Stripping and regalvanizing costs time but restores a full metallurgical coating. On overseas work it should always happen before shipment, because the same decision on site means a repair far from any kettle.

Repairs before duplex painting

When galvanized steel will be painted, repaired areas need the same attention as the rest of the surface. Zinc-rich paint repairs must be compatible with the paint system that follows, and metallized or soldered repairs are prepared with the rest of the zinc. The paint manufacturer's data sheet decides which repair products can be overcoated, which is one more reason to list the repair method on the coating schedule.

Reading a repair on a coating report

When a repaired piece reaches a reviewer, three questions decide whether the repair is acceptable: was each area within 25 mm (1 in) in its narrowest dimension, was the total within the Section 6.2.2 limit for that piece, and was the repair measured at the Section 6.2.3 thickness. A report that answers all three by piece mark, with a photograph before and after, needs no further explanation.

How World Steel handles galvanizing repairs

World Steel fabricates up to 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam. Galvanizing is arranged in Vietnam with a galvanizer named for the job, under our written galvanizing procedure with the tighter repair limits above. Every repaired area is logged with its size, method and thickness, and the repair records go into the submittal with the thickness readings and the certificate of conformance, posted in PEB Studio by piece mark.

For site damage, we ship a touch-up procedure naming the A780 method and the product. Finish and appearance rules are covered in galvanized coating finish and appearance, and what happens when a lot fails in galvanizing inspection, rejection and retest. For the standard at a glance, see our ASTM A123 page.

Quick answers

How large an area of galvanizing may be repaired under ASTM A123?

Each area must be 25 mm (1 in) or less in its narrowest dimension, and the total on each article no more than 0.5 % of the accessible surface to be coated, or 256 cm² per metric ton of piece weight (36 sq in per short ton), whichever is less.

What are the ASTM A780 repair methods?

Zinc-based solders applied to the heated surface, paints containing zinc dust (zinc-rich paints), and sprayed zinc (metallizing). The galvanizer or the repairer chooses the method, unless the purchaser specifies one.

How thick must a galvanizing repair be?

The Table 1 thickness for the material category and steel thickness. For zinc-rich paint, Section 6.2.3 requires 50 % more than Table 1, but not more than 100 µm (4.0 mils).

Who repairs damage after erection?

The US contractor, our customer, as part of the site work, using an ASTM A780 method and the repair product listed in the submittals. Damage in transit or erection is not covered by the galvanizer's A123 limits, which apply to shipment from the galvanizer.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

ASTM A123 hot-dip galvanizing series

Sixteen in-depth articles that follow a galvanized member from the coating specification, through design for the kettle and the dip itself, to the thickness gauge, the repair rules and the jobsite. Each one explains a part of ASTM A123 in plain terms and lists what to check.

Specify and order

What A123 covers, what goes on the order, and the steel and zinc chemistry behind the coating.

Design for the kettle

Vent and drain holes, distortion, embrittlement and welded assemblies.

Through the kettle

The hot-dip process step by step and the zinc-iron layers it grows.

Thickness and sampling

Coating grades by steel, how the zinc is measured and how a lot is sampled.

Finish, repair and the site

What the finish may show, A780 repairs, inspection and retest, and storage on the way to the job.

Bidding a large US project?

Send the bid documents, or just a footprint and an address. Our engineers check them against US code requirements and confirm what World Steel would supply, from a plant that fabricates 2,500 metric tons of structural steel a month.