Close view of galvanized ring assemblies showing the zinc finish

Coatings and durability

Galvanized coating finish and appearance: what may be rejected and what may not

Galvanized steel never looks like paint, and it is not meant to. The rules on galvanized coating finish in ASTM A123 separate real defects from the normal look of zinc. Here is how to tell them apart before a lot is rejected.

· 7 min read · World Steel USA engineering team

The first thing anyone notices about a galvanized member is how it looks, and the first argument on a galvanized job is usually about it. Galvanizing is not paint: its finish varies with the steel, the shape and the process, and ASTM A123 is written to separate real defects from the normal look of zinc. This article goes through the rules on galvanized coating finish and appearance in Sections 6.2 to 6.5, with the features an inspector should and should not reject.

The edition reviewed is ASTM A123/A123M-13. The edition your specification names governs.

The finish rule in one paragraph

Section 6.2 requires the coating to be continuous, apart from the renovation allowed below, and as reasonably smooth and uniform in thickness as the weight, size and shape of the item, and the handling needed during dipping and draining, will permit. Rejection for nonuniform coating is made only for plainly visible excess coating that is not related to design factors such as holes, joints or special drainage problems, except for local excess coating that would interfere with the use of the product or make it dangerous to handle, such as edge tears or spikes.

Two key ideas follow. The finish is judged against what the piece allows, not against a perfect surface. And excess zinc is a defect only when it is plainly visible and unrelated to the design, or when it gets in the way of use or safety.

What is not a defect

Section 6.2 lists three kinds of roughness that are not grounds for rejection:

  • Minor roughness that does not interfere with the intended use of the product.
  • Roughness related to the as-received surface of the steel before galvanizing, such as pitting, rolled-in scale marks or a blasted surface. Note 7 adds that steel prepared by abrasive cleaning generally develops a thicker coating with a moderately rougher surface.
  • Roughness related to steel chemistry or reactivity to zinc, which also brings the matte gray finish explained in reactive steel and the zinc bath.

Section 6.2 adds a fourth: surface conditions related to deficiencies of design, detailing or fabrication, as addressed by ASTM A385, are not grounds for rejection of the coating. If zinc pooled because a pocket had no drain hole, the remedy lies with the detailing, as vent and drain holes for galvanizing explains.

Note 6 completes the picture: the finish requirements are about visual inspection, not about the measured thickness differences that come from different steels or thicknesses in one assembly.

What must not be there

Section 6.4 lists what galvanized articles must be free of when they leave the galvanizing facility:

Feature What it looks like Usual cause
Uncoated areas Bare steel, often with a dark or rusty edge Slag, paint, oil or scale not removed; air trapped
Blisters Raised bubbles in the zinc Gas from the steel or trapped liquids
Flux deposits Dark, crusty or powdery patches Wet or contaminated flux, poor drying
Gross dross inclusions Raised lumps of zinc-iron alloy Dross picked up from the bath

Section 3.2.4 explains why gross dross matters: it is zinc-iron alloy present in a form other than finely dispersed pimples, raised and easily knocked off by slings, chains, tools, fixtures or other parts, and it would leave an exposed steel spot if removed. Fine dross pimples, by contrast, are part of normal galvanizing.

Section 6.4 also forbids lumps, projections, globules or heavy deposits of zinc that will interfere with the intended use of the material. A drip on the underside of a beam flange is cosmetic; a lump on a bearing face, a faying surface or a handrail is not.

Holes and threads

Two rules deal with the places where excess zinc causes trouble at erection.

Holes. Section 6.4 requires plain holes of 12.5 mm (1/2 in) diameter or more to be clean and reasonably free from excess zinc. Note 8 explains that, depending on design and material thickness, filming or excess zinc may build up in smaller holes and need extra work to make them usable. On structural steel, most bolt holes are larger than 12.5 mm and should arrive clear; small holes in light members may need reaming or punching through on site.

Threads. Section 6.2 and Section 6.3 say the zinc on threaded components of A123 articles must meet ASTM A153. External threads must not be cut, rolled or finished with a tool unless the purchaser authorizes it, while internal threads may be tapped or retapped after galvanizing. Welded studs and threaded rods are usually cleaned by brushing after galvanizing so nuts run on.

Handling marks and pieces stuck together

Galvanizers hold steel with wire, hooks, chains and tongs. Section 6.4 says marks in the coating caused by tongs or other items used in handling during galvanizing are not cause for rejection, unless they have exposed the base metal and the bare areas exceed the limits of Sections 6.2.1 and 6.2.2. Small contact marks at hanging points are normal and are repaired where they are bare.

The same section requires pieces to be handled so that after galvanizing they do not freeze together on cooling. Small parts dipped in baskets, and moving parts on assemblies, are the usual risk.

Adherence

Section 6.5 sets the last coating property: the zinc must withstand handling consistent with the nature and thickness of the coating and the normal use of the article, without peeling or flaking. Note 9 warns that the coating is generally too heavy to allow severe bending without damage. Where adherence is in question, Section 8.3 gives the knife test: a stout knife is pressed into the coating with considerable pressure in a way that tends to remove a portion of it. Adhesion is inadequate if the coating flakes off as a layer and exposes the base metal ahead of the knife point. Edges and corners are not used for the test, and removing small particles by paring or whittling is not a failure.

Features that often cause needless arguments

Some features look alarming but are normal or cosmetic:

  • Spangle, the crystal pattern on bright zinc, and its absence on other steels.
  • Dull gray or mottled areas, from steel chemistry.
  • Runs and drip lines at the lower end of a member, from drainage during withdrawal.
  • Zinc ash, a light gray powdery deposit picked up from the bath surface, which brushes off and leaves sound zinc underneath; heavy ash lumps are another matter.
  • Rust staining weeping from a lap or a seam, which comes from trapped liquid, not from failed zinc, and is a detailing issue.
  • White powder after storage, which is wet storage stain, covered in wet storage stain on galvanized steel.

Architectural expectations

On exposed architectural steel, owners sometimes expect a uniform, bright finish. ASTM A123 does not promise one, and the steel may not allow it. The practical options are to agree an appearance standard with the owner before fabrication, for example a reference sample, to keep the steel source consistent, to specify grinding of drips on visible faces, or to use a duplex paint system where color uniformity matters. Those are special requirements under Section 4.1.7, so they belong on the order.

A visual inspection routine

A practical routine for each lot:

  1. Check every piece for uncoated areas, blisters, flux and gross dross.
  2. Look at bearing faces, faying surfaces and handrail for lumps and spikes.
  3. Check plain holes of 12.5 mm (1/2 in) and larger are clear.
  4. Check threads run free and studs are clean.
  5. Measure any bare area against the repair limits.
  6. Do not reject for gray zinc, minor roughness or handling marks within limits.

Who decides when the finish is in doubt

Finish is judged by eye, and two people can see the same surface differently. Three habits reduce disputes:

  • Agree reference samples for exposed steel before fabrication, photographed and kept with the job records.
  • Judge in good light at a normal viewing distance for the use of the part, not with a lamp at a raking angle.
  • Separate appearance from performance: ask first whether a feature interferes with use, safety or later painting, then whether it is one of the four Section 6.4 defects.

When a lot is rejected on visual grounds, Section 9.4 lets the galvanizer sort it, remove the nonconforming pieces and submit it again with the same sampling plan, so one bad piece does not condemn the whole lot. Rejected pieces can be repaired within the limits of Section 6.2 or stripped and galvanized again.

Finish and duplex painting

If the steel will be painted, the finish matters for a different reason: high spots, drips and zinc ash must be removed so the paint can build evenly, and the steel must not have been passivated. The order should name the members to be painted, and the galvanizer grinds drips and spikes flush before release. The paint preparation itself follows SSPC-SP 16 or the paint maker's instructions.

Photographs as part of the record

A photograph of each defect type found, with its piece mark and disposition, turns a visual judgment into evidence. On overseas work it also lets the purchaser's inspector review a borderline case remotely before the steel ships, rather than after it arrives. We attach photographs to nonconformance reports as a matter of routine.

How World Steel inspects the finish

World Steel fabricates up to 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam. Galvanizing is arranged in Vietnam with a galvanizer named for the job, under our written galvanizing procedure, and every piece is inspected visually for bare spots, burns, drips, inclusions and white rust before thickness is measured. Drips are filed or ground smooth, hanging-wire marks are touched up, and holes and threads are checked before release.

Defects are logged on a nonconformance report and held aside until dispositioned, and anything beyond the repair limits is stripped and dipped again. Repairs are covered in repairing galvanized coatings. See the procedure on our hot-dip galvanizing page and the standard at a glance on our ASTM A123 page.

Quick answers

What finish defects can reject galvanized steel under ASTM A123?

Uncoated areas, blisters, flux deposits and gross dross inclusions when the steel leaves the galvanizer, plus lumps, projections or heavy zinc that interfere with the use of the part, and edge tears or spikes that make it dangerous to handle.

Is rough or gray galvanizing a defect?

Not by itself. Section 6.2 says minor roughness that does not interfere with use, roughness from the as-received steel surface, and roughness from steel chemistry or reactivity are not grounds for rejection.

Must bolt holes be free of zinc?

Plain holes of 12.5 mm (1/2 in) diameter or more must be clean and reasonably free of excess zinc. Smaller holes may fill or film with zinc and need extra work, as Note 8 explains.

Are tong or hook marks a defect?

No, unless they expose bare steel over areas larger than the repair limits of Sections 6.2.1 and 6.2.2. Small marks from handling during galvanizing are normal.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

ASTM A123 hot-dip galvanizing series

Sixteen in-depth articles that follow a galvanized member from the coating specification, through design for the kettle and the dip itself, to the thickness gauge, the repair rules and the jobsite. Each one explains a part of ASTM A123 in plain terms and lists what to check.

Specify and order

What A123 covers, what goes on the order, and the steel and zinc chemistry behind the coating.

Design for the kettle

Vent and drain holes, distortion, embrittlement and welded assemblies.

Through the kettle

The hot-dip process step by step and the zinc-iron layers it grows.

Thickness and sampling

Coating grades by steel, how the zinc is measured and how a lot is sampled.

Finish, repair and the site

What the finish may show, A780 repairs, inspection and retest, and storage on the way to the job.

Bidding a large US project?

Send the bid documents, or just a footprint and an address. Our engineers check them against US code requirements and confirm what World Steel would supply, from a plant that fabricates 2,500 metric tons of structural steel a month.