"How thick is the zinc?" is the first question an engineer asks about galvanized steel, and ASTM A123 does not answer it with one number. The ASTM A123 coating thickness requirement depends on the kind of steel, its thickness, the size of the piece and how the readings are averaged. Get those four things right and the coating schedule writes itself; get one wrong and an inspector can reject a fully compliant lot, or accept one that is not. This article explains how the grades work.
The edition reviewed is ASTM A123/A123M-13, and the values below are a selection from its Table 1 for the steel most structural jobs use. The full table, including wire and reinforcing bar, is in the standard, and the edition your specification names governs.
Grades, not just micrometres
Section 3.2.3 defines the coating thickness grade as the number in Table 1 at the meeting point of a material category and a steel thickness range. Table 2 then gives each grade in four units. The grade number equals the thickness in micrometres, so grade 100 is 100 µm. The other units follow fixed conversion factors given in the note to Table 2: mils are µm × 0.03937, ounces per square foot are µm × 0.02316 and grams per square metre are µm × 7.067.
| Coating grade | Micrometres | Mils | g/m² |
|---|---|---|---|
| 45 | 45 µm | 1.8 | 320 |
| 65 | 65 µm | 2.6 | 460 |
| 75 | 75 µm | 3.0 | 530 |
| 100 | 100 µm | 3.9 | 705 |
Section 6.1 says that for SI orders the Table 1 values apply directly as micrometres, and for inch-pound orders the measured value is converted to a grade using Table 2. Either way the grade is what is judged.
Material category
Section 3.2.5 defines the material category as the general class or type of material, or the process of manufacture, that describes the product. Table 1 has six: structural shapes, strip and bar, plate, pipe and tubing, wire, and reinforcing bar. The definition gives two useful examples: bar grating belongs to strip, and handrail belongs to pipe.
On a structural job the usual mapping is:
- Structural shapes: wide flange beams and columns, channels, angles, tees and welded built-up members.
- Plate: base plates, cap plates, gussets, stiffeners and connection plates.
- Strip and bar: flat bar, round bar, bar grating and stair treads.
- Pipe and tubing: hollow structural sections, pipe columns, handrail and tube bracing.
Steel thickness
Each category has six thickness ranges, from under 1.6 mm (1/16 in) to over 16 mm (5/8 in). The thickness is the measured steel thickness, not the nominal section size. For a wide flange, the flange and the web may fall in different ranges.
For the two categories that matter most on structural frames, the 2013 edition gives:
| Measured steel thickness | Structural shapes | Plate |
|---|---|---|
| 3.2 to 4.8 mm (1/8 to 3/16 in) | 75 µm (3.0 mils) | 75 µm (3.0 mils) |
| 6.4 to under 16.0 mm (1/4 to under 5/8 in) | 100 µm (3.9 mils) | 75 µm (3.0 mils) |
| 16.0 mm (5/8 in) and over | 100 µm (3.9 mils) | 100 µm (3.9 mils) |
Thinner steel needs less: 65 µm (2.6 mils) from 1.6 mm (1/16 in) and 45 µm (1.8 mils) below that, for these categories. Pipe and tubing stays at 75 µm (3.0 mils) from 3.2 mm (1/8 in) upward. Our coating grade finder shows every combination for shapes, plate, bar and tubing.
What changed in 2013
The Summary of Changes at the end of A123/A123M-13 records one change that still causes confusion. Earlier editions had a single line for "structural shapes and plate". The 2013 edition split it into two lines. Structural shapes kept their requirements, but the requirement for plate up to 16 mm (5/8 in) thick was reduced, because of steelmaking practices and chemistries. That is why plate from 6.4 to under 16 mm (1/4 to under 5/8 in) needs 75 µm (3.0 mils) while a shape of the same thickness needs 100 µm (3.9 mils).
An inspector working from an older edition would apply 100 µm (3.9 mils) to that plate and could reject it wrongly. Naming the edition on the order, as Section 4.1.3 requires, prevents it.
Specimens: one piece, one or three areas
Thickness is judged per specimen, the surface on which readings are taken. Section 3.2 sets two cases by surface area, with 100,000 mm² (160 sq in) as the dividing line:
- A single-specimen article has a surface area of 100,000 mm² (160 sq in) or less, or is spun in a centrifuge. The whole surface is one specimen.
- A multi-specimen article is larger. It is divided into three continuous local sections of about equal surface area, and each is a specimen.
If an article, or one of its three sections, contains more than one material category or thickness range, it contains more than one specimen, one for each. A welded frame with a 20 mm flange, a 10 mm web and a 12 mm end plate is judged as several specimens, each against its own line of the table.
Section 3.2.10 defines the specimen coating thickness as the average of at least five readings on the specimen, placed to spread as widely as possible across it. Section 3.2.9 excludes areas affected by flame cutting, machining or threading from magnetic measurements, because they are not representative of the general surface.
The one-grade-lower rule
Section 6.1 has two levels of requirement:
- The average of all specimens tested must meet the Table 1 grade.
- Any individual specimen may be one coating grade below it.
For multi-specimen articles, Section 6.1.1 applies the rule per test article: each test article must meet the Table 1 average, and each specimen making up that average must be no more than one grade below. For single-specimen articles, Section 6.1.2 applies it to the sample: the average of all test articles must meet Table 1, and each test article must be no more than one grade below.
"One grade below" means the next lower grade in Table 2. For grade 100 that is grade 85, 85 µm (3.3 mils); for grade 75 it is grade 65; for grade 65 it is grade 60; for grade 45 it is grade 35.
Single low readings do not reject
Section 6.1.3 adds a rule that inspectors sometimes forget. No individual reading, or cluster of readings in the same general location, is a reason for rejection as long as the average of those readings with the other dispersed readings meets the requirement for the specimen. The gauge is used to find the average, not to hunt for the thinnest point.
Note 4 explains why. The Table 1 grades are minimum values that can be reached with a high level of confidence for the range of steels in each category. Most coatings will be thicker, but some steels are less reactive, because of chemistry or surface condition, and may come out close to the minimum. In those cases the precision and accuracy of the measuring method should be considered before rejecting.
Asking for more zinc
Purchasers can ask for a heavier coating, but Note 4 sets expectations. A guarantee of a heavier coating should be written as a special requirement under Section 4.1.6, and the purchaser should expect test batches or extra preparation, such as abrasive blasting before galvanizing, to reach it consistently. Some higher thicknesses may be impractical or unattainable. Note 7 adds that blasting before galvanizing generally develops a thicker coating with a moderately rougher surface.
If a project needs a longer coating life than the Table 1 minimum gives, a duplex paint system over the galvanizing is often the more reliable route. The choice is covered in paint, galvanizing or duplex.
Writing grades on a coating schedule
A clear schedule lists, for each galvanized member type:
- Piece mark range and description.
- Material category under Table 1.
- Measured steel thickness of each part.
- Minimum average coating grade in µm, with mils.
- Any heavier grade agreed under Section 4.1.6.
- The A123 edition, for example A123/A123M-13.
That is the list we send with our shop drawings for galvanized work.
Reading the grade on a mixed assembly
Most galvanized pieces on a structural job are not single shapes. A column with a base plate, cap plate and stiffeners combines two material categories and several thicknesses. Under Section 3.2.9 each one is its own specimen, so the column is judged as several specimens, each against its own line:
| Part of the column | Category | Thickness | Minimum average grade |
|---|---|---|---|
| Column flanges | Structural shapes | 14 mm | 100 µm (3.9 mils) |
| Column web | Structural shapes | 9 mm | 100 µm (3.9 mils) |
| Base plate | Plate | 25 mm | 100 µm (3.9 mils) |
| Stiffeners | Plate | 10 mm | 75 µm (3.0 mils) |
| Cap plate | Plate | 12 mm | 75 µm (3.0 mils) |
Because the column is larger than 100,000 mm² (160 sq in), it is also split into three local sections, and each section contains its own specimens for each part it includes. That sounds complicated, but in practice an inspector simply reads each kind of surface separately, records it under the right line and averages within each.
Why thicker steel gets more zinc
The grades rise with steel thickness for a physical reason. A thick member takes longer to reach bath temperature, so it stays in the zinc longer and the alloy layers keep growing. Thick members also hold heat after withdrawal, so the reaction continues for a while. The Table 1 grades reflect what the process reliably produces on each thickness range, which is why thin sheet-like parts have the lowest minimums.
It also explains a common surprise. On a welded assembly, the thin parts often come out closer to their minimum and the heavy parts well above theirs, because the whole piece spends the same time in the bath. Specimen-by-specimen judging under Section 3.2.9 is the standard's answer to that.
Grades and coating life
ASTM A123 does not give a coating life, and the grades are not a life rating. How long zinc lasts depends on the exposure: dry interiors consume almost nothing, while marine and industrial air consume zinc much faster. The grade sets the minimum zinc on the steel; the corrosivity of the site, often stated as an ISO 12944 category, decides how fast it is used. That is why a coating schedule for an exposed coastal structure often adds a duplex paint system rather than relying only on a heavier grade.
How World Steel checks coating thickness
World Steel fabricates up to 2,500 metric tons of structural steel a month in its own IAS AC472-accredited plant in Vietnam. Galvanizing is arranged in Vietnam with a galvanizer named for the job, under our written galvanizing procedure, and every lot is read with an Elcometer 456 magnetic gauge against Table 1 for each material category and thickness on the piece. The readings are recorded per specimen and averaged as Section 6.1 requires, so your inspector sees the same arithmetic the standard uses.
How the readings are taken, and the other three methods A123 allows, are covered in measuring galvanized coating thickness. For the coating grade of any member, use the finder on our ASTM A123 page.
Quick answers
What is the minimum galvanized coating thickness for structural steel?
Under ASTM A123/A123M-13, structural shapes 6.4 mm (1/4 in) and thicker need a minimum average coating grade of 100, which is 100 µm (3.9 mils). Thinner shapes need 75 µm (3.0 mils), 65 µm (2.6 mils) or 45 µm (1.8 mils), depending on thickness.
Can one specimen be thinner than the table value?
Yes, by one coating grade. Section 6.1 allows any individual specimen to be one grade below the Table 1 value, as long as the average for the article, or for the sample of small parts, meets it.
What changed for plate in the 2013 edition?
Table 1 was split so structural shapes and plate have separate lines. The minimum for plate up to 16 mm (5/8 in) thick was reduced to 75 µm (3.0 mils), reflecting steelmaking practices and chemistries, while structural shapes stayed at 100 µm (3.9 mils) from 6.4 mm (1/4 in).
How do coating grades convert to other units?
Under Table 2 the grade equals the thickness in micrometres. Mils are µm × 0.03937, oz/ft² are µm × 0.02316 and g/m² are µm × 7.067, with the table giving rounded values.
Keep building your steel plan
Go further on USPEB.com
On this topic
Across the US market
- Steel fire protectionIntumescent and fire-rated steel packages
- Quality hubCoating inspection by FROSIO Level III inspectors
- Products catalogGalvanized, painted and built-up members
- Download centerSample ITP, design report and approval drawings
- Large projects, 2,500 t a monthCapacity for large US general contractors
- Contractor partnershipLong-term supply for US contractors