Skip to content
Seeking US contractor partners IAS AC472 ACCREDITED ★ METAL BUILDINGS ★ AC472 IAS AC472 accreditedIAS AC472
World Steel USA
Steel plates stacked and labelled in the World Steel plate store

Quality and certification

Seismic base metal repair: grinding tapers and repair welding under AWS D1.8

Gouges, arc strikes, misplaced tacks and cutting notches happen in every shop. In a seismic frame each one is a possible crack starter, so AWS D1.8 sets exactly how they are ground out or welded back. Here are the two repair routes and when each applies.

· 7 min read · World Steel USA engineering team

No steel shop delivers members that never needed a repair. A torch wanders and leaves a gouge. An arc strikes the flange where it shouldn't. A tack weld lands in the wrong place, a saw overruns, a lifting chain bites into an edge. On a gravity beam most of these are cosmetic. On a member of a seismic force-resisting system (SFRS), and above all inside a Protected Zone, every one of them is a notch that can start a crack when the steel yields. AWS D1.8 handles this with one short clause, Clause 6.19, that the rest of the code points back to again and again. This article explains seismic base metal repair under that clause: the grinding route, the welding route, and the places in the code that call for each.

One clause, many callers

Clause 6.19 is the common repair standard for D1.8. It is called from:

  • Clause 6.11.2, weld access hole notches and gouges
  • Clause 6.12.4, misplaced tack welds
  • Clause 6.13, backgouged roots and notches left after backing removal
  • Clause 6.16.3, defects at weld tab removal sites
  • Clause 6.18.5 to 6.18.8, gouges, notches, mislocated holes and fasteners in the Protected Zone

So a shop that gets Clause 6.19 right gets a large part of D1.8 right. Each calling clause sets when a repair is needed and sometimes adds its own limit; Clause 6.19 sets how the repair is made.

Route one: grinding (Clause 6.19.1)

When a surface is repaired by grinding, the area is either ground flush or ground to give a gradual taper:

Direction Maximum slope
Parallel to the member axis 1:5
Transverse to the member axis 1:2.5

A 1:5 taper means the ground surface rises 1 mm for every 5 mm of length. For a notch 2 mm deep along a beam flange, the ground dish needs to run about 10 mm each side of the deepest point in the axial direction, and about 5 mm across.

The commentary to Clause 6.18.5.1 explains the two slopes. A stress concentration perpendicular to the applied stress is more severe than one parallel to it. Shop drawings rarely show which way stress flows, but anyone can see the member axis, so the code assumes the main stress runs along the axis and requires the gentler slope in that direction.

Grinding is the preferred repair wherever it works. It adds no heat, no weld metal, no hydrogen and no new chance of a weld defect. The commentary on access holes says this directly, and good shops apply it everywhere. Some calling clauses limit depth through tolerance: an access hole, for example, must still meet its required dimensions after grinding.

Route two: repair welding (Clause 6.19.2)

When grinding alone cannot restore the surface within the limits, the repair is welded. Clause 6.19.2 sets six steps:

  1. Prepare the cavity. Grind the surface to give a smooth radius of at least 6 mm (1/4 in), so the welder can fuse the bottom and sides.
  2. Use a WPS. Weld in accordance with an applicable welding procedure specification.
  3. Preheat. Minimum preheat follows AWS D1.1 but is never less than 66 °C (150 °F), even where D1.1 would allow less.
  4. Use the right electrodes. Filler metal must meet Clause 6.1, the D1.8 filler metal requirements for SFRS welds.
  5. Finish. Grind the repair weld to a smooth contour, with surface roughness no more than 13 µm (500 µin). AWS C4.1 sample 4 may be used as a guide.
  6. Inspect. Test the repaired area by magnetic particle testing (MT).

Clause 6.19.2 closes with a thickness rule: the finished repaired area must be at least the base metal thickness less 1.5 mm (1/16 in).

The commentary to Clause 6.18.5.2 explains the extra care. Repairs are usually made under high restraint, a small weld in a large, cold piece of steel, so more preheat is needed to avoid hydrogen cracking. MT is used because the main risk is a surface-breaking crack in or beside the repair. The grinding slope limits still apply to the finished repair, whether it ends up slightly below the surface or as a small mound above it. The WPS may be prequalified even though the repair cavity is not a prequalified joint shape, as long as the cavity gives the welder enough access.

Why preheat of at least 66 °C

A small repair weld cools very quickly because the surrounding steel draws heat away from it in every direction. Fast cooling produces a hard heat-affected zone, and a hard zone combined with hydrogen and restraint is the recipe for cold cracking. D1.1 preheat tables are based on the thickness and steel grade, and for thin parts they can call for very low or no preheat. D1.8 sets a 66 °C floor for repairs regardless, as a margin for that rapid cooling. On thick or high-carbon-equivalent steel, the D1.1 value or the WPS value will be higher and governs.

Choosing the route

The choice between grinding and welding usually comes down to three checks:

  1. Depth against thickness. If grinding out the defect would leave less than the base metal thickness less 1.5 mm, or break a tolerance such as an access hole dimension, grinding alone cannot work.
  2. Room for the taper. A 1:5 slope along the axis needs space. Next to a weld toe, a hole or a plate edge there may not be enough length to fair the dish out.
  3. What the calling clause allows. Some clauses set a depth limit for grinding, such as the 1.5 mm limit after back welding or at weld tab sites; past it, the repair must be welded.

If all three pass, grind. If any one fails, weld under Clause 6.19.2.

The calling clauses in detail

Access holes (6.11.2). Notches and gouges are ground out to 1:5 on straight cuts or to at least a 10 mm radius on curves, within the hole's tolerances. Deeper ones are repaired by welding under Clause 6.19.2. The commentary adds that the welded area must be ground to sound metal, not only smooth. Clause 7.7 requires MT or penetrant testing (PT) of access hole repairs in a Protected Zone. See our article on weld access holes.

Tack welds (6.12.4). Misplaced tacks are removed by grinding. Gouges and notches are repaired regardless of dimensions, by grinding or welding at the contractor's choice.

Backing removal (6.13). After backing is removed, the root is backgouged to sound metal and restored by welding under Clause 6.19.2. Notches no deeper than 1.5 mm left after back welding are ground under Clause 6.19.1; deeper ones are welded. See our article on weld backing removal.

Weld tab removal (6.16.3). Defects at the weld end no deeper than 1.5 mm are ground; others are excavated and welded. Clause 7.8 then requires MT of the repaired area and the area around it. See our article on weld tab removal.

Protected Zone (6.18). Gouges and notches are ground under Clause 6.19.1 or welded under Clause 6.19.2. Mislocated holes and mislocated screws or shot pins that the Engineer wants weld-restored need a contractor procedure approved by the Engineer, restoration under Clause 6.19.2 and then ultrasonic testing (UT). Mislocated studs are cut off and ground flush. See our article on protected zone fabrication rules.

Arc strikes

D1.8 relies on D1.1 for arc strikes. D1.1 requires arc strikes outside the weld to be avoided, and any cracks or blemishes they cause to be ground to a smooth contour and checked for soundness. In an SFRS member the practical approach is the same as for any other notch: grind the strike smooth to the Clause 6.19.1 tapers, check that the hard spot is gone, and treat any crack found as a repair under Clause 6.19.2. Arc strikes most often come from a stray electrode touching the steel or a poor ground clamp connection, so prevention starts with grounding directly on the piece being welded.

A repair record that holds up

Seismic repairs are often reviewed months later by the Engineer, the special inspector or the owner's representative. A good repair record shows:

  • the piece mark and exact location, with a sketch or photo
  • what was found and how it was measured
  • the route chosen, grinding or welding, and why
  • for welding: the WPS, welder, preheat reading, filler metal lot and MT result
  • for grinding: the final depth and taper, and remaining thickness
  • who accepted the repair and when

Where a repair needs the Engineer's approval, such as mislocated hole restoration, the approved procedure and the UT report go in the same record.

Common repair mistakes

  • Steep grinding. A deep notch ground out as a narrow, steep-sided trench is still a notch. The slope rule matters as much as removing the defect.
  • Skipping preheat on small repairs. The 66 °C floor applies to the smallest repair.
  • Welding into a sharp-bottomed cavity. Without the 6 mm radius, the root of the repair is likely to lack fusion.
  • Leaving the weld as deposited. A repair weld not ground to 13 µm leaves its own toe notches.
  • No MT. Every Clause 6.19.2 repair is MT tested; it is not optional.
  • Over-grinding. Grinding below the base metal thickness less 1.5 mm means the repair has created a new nonconformance.

How World Steel handles repairs

At World Steel, any defect found on an SFRS member is logged as a nonconformance, with the repair route decided by QC against the rules of AWS D1.8 Clause 6.19 and the contract documents. Grinding is used wherever the tapers allow; welded repairs follow a qualified WPS with preheat checked and recorded, and are MT tested afterwards. Our shop welding procedures and welders are qualified to AWS D1.8, and each repair is recorded with its piece mark in our IAS AC472-accredited quality system, where the special inspector can review it through inspector access. Our nonconformance control page explains how repairs are tracked to closure.

Quick answers

How steep can a ground repair be?

No steeper than 1:5 in the direction of the member axis and 1:2.5 across it, under Clause 6.19.1. The area may also be ground flush.

What does a repair weld need under Clause 6.19.2?

A ground cavity with at least a 6 mm (1/4 in) radius, an applicable WPS, preheat of at least 66 °C (150 °F), electrodes meeting Clause 6.1, grinding to 13 µm (500 µin) afterwards and MT of the finished repair.

How thin can the repaired area be?

At least the base metal thickness less 1.5 mm (1/16 in).

Which repair is preferred, grinding or welding?

Grinding, where the slope and dimension limits allow it. It adds no heat, no new weld metal and no new chance of defects.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

AWS D1.8 seismic fabrication series

Twenty in-depth articles that follow a seismic weld from the drawings to the last test report. Each one explains a part of AWS D1.8:2025 in plain terms and lists the checks a general contractor can ask the fabricator about.

Drawings and scope

What the code covers, which welds are Demand Critical, and the data the drawings must carry.

Procedures and welders

The WPS, the restricted access welder test and the bottom flange sequence.

Details and Protected Zones

Access holes, backing, weld tabs, k-area details, Protected Zones and repairs.

Inspection and testing

Who inspects what, inspector qualifications, and UT and MT done the D1.8 way.

Bidding a large US project?

Send the bid documents, or just a footprint and an address. Our engineers check them against US code requirements and confirm what World Steel would supply, from a plant that fabricates 2,500 metric tons of structural steel a month.