Most complete joint penetration (CJP) groove welds in a seismic moment frame cannot be inspected inside by eye. A flaw buried in the root of a beam flange weld, or hidden behind steel backing, can only be found by ultrasonic testing (UT). After the 1994 Northridge earthquake, investigators found that many fractured joints had root flaws that UT had missed, and SAC and FEMA studies showed a wide spread in the skill of UT technicians. AWS D1.8 Clause 7.10 and Annexes F, G and H respond with tighter procedures, a hands-on qualification for technicians, an optional flaw sizing route and a defined method for magnetic particle testing (MT). This article explains ultrasonic testing of demand critical welds and the supporting MT rules, in the order an inspector applies them.
Why UT needed tightening
The D1.8 commentary to Clause 7.2.4 is direct about the problem. UT technicians are usually certified by their own employer under ASNT SNT-TC-1A, and Level II requirements vary a lot from one organization to the next. ASNT Level III technicians are not required to pass a hands-on practical test. Research cited in the commentary showed that technicians often had difficulty evaluating flaws near steel backing. In a joint where the most dangerous flaw is at the root, next to the backing, that is a serious gap.
D1.8 addresses it from two sides: the procedure must be proven to cover the joint, and the technician must be proven to find flaws in it.
A qualified, joint-specific procedure
Clause 7.10.1 requires UT of welds called for by the QAP to follow the procedures of AWS D1.1 Clause 8, Part F, using a written procedure containing the elements of D1.1 Annex N, Clause N3. Those Part F procedures must be qualified using weld mockups with 1.5 mm diameter side drilled holes, similar to D1.1 Annex N Figure N.3.
The commentary explains the intent. The procedure must be specific to the Demand Critical joints being tested, and the mockup proves that the sound beam reaches the whole weld volume, especially the places that are hard to reach. The side drilled holes are placed where it is difficult to direct sound, and an ASNT Level III technician decides how many holes and mockups are needed. The commentary's main example is a T-joint with steel backing: the procedure may need to show full root coverage from a third-leg scan from one side, or show how reflections from the backing are interpreted.
Acceptance criteria
Clause 7.10.2 sets the criteria for flaw detection:
- welds tested with the D1.1 Clause 8 Part F procedures are judged to D1.1 Table 8.2
- where the Engineer approves the alternative techniques of D1.1 Annex N, welds are judged to Annex N Table N.1, Weld Class S (statically loaded structures)
The commentary notes that alternative techniques can give more information about the size, location and nature of embedded flaws, but they need equipment calibrated on standard reflectors to set a standard sensitivity level and disregard level.
Left-in-place backing and PJP roots
Two rules prevent automatic rejection where UT physics, not weld quality, produces the signal:
- Left-in-place steel backing (7.10.4). Joints are not rejected on the indication rating of geometric reflectors caused by backing. The commentary warns that this works both ways: a sound weld with backing gives reflections that look like flaws, and a real flaw can be dismissed as a backing reflection. D1.1 guidance on welds with steel backing helps the technician tell them apart.
- PJP groove welds (7.10.5). When UT of partial joint penetration welds is required, rejection is not based on the indication rating from the unfused weld root, which is part of the design.
Our article on weld backing removal explains why backing is removed at bottom flange joints, which also removes this source of confusion.
Annex F: proving the technician
Clause 7.2.4 requires every UT technician doing QA on these welds to be Level II or III by employer certification, or ASNT Level III by examination, and certified by the employer under Annex F. The Annex F exam works as follows:
- Exam content (F2). Practical tests written by the NDT agency's UT Level III, or an approved organization, using the agency's procedures and the D1.8 acceptance criteria. The exam also tests calibration and paperwork, and results are documented for the Engineer.
- Test specimens (F3). Mockups of typical butt and T-joints, with and without steel backing, containing natural flaws or artificial ones such as non-metallic inserts or thin steel inserts that simulate incomplete fusion. Each flaw is confirmed by RT or UT, and two Level III technicians must agree on its classification.
- Number of flaws. At least 20 flaws per candidate, spread over several plates. Flaw details are kept confidential so the plates can be reused.
- Reporting (F4.1). The candidate reports every indication with its rating in decibels, length, location along the weld and position in the cross-section.
A reported indication counts as a detected flaw if at least two of these match the true flaw within tolerance:
| Attribute | Tolerance |
|---|---|
| Indication rating | ±6 dB |
| Length | +25 mm to −12 mm (+1 in to −0.5 in) |
| Depth | ±6 mm (±0.25 in) |
The score combines the detection rate D (detected flaws divided by total flaws) and the false call rate F (false indications divided by total indications) into a rating R = ½ (1 + D − F). To qualify, the candidate needs R ≥ 0.90, D ≥ 0.87 and F ≤ 0.15. A technician who has not done UT on steel construction for 6 months or more must requalify (F5).
The commentary recommends third-party examination, because realistic flaw mockups are expensive to make and a shared set gives consistent, comparable results across technicians.
Annex H: when a weld fails UT
Clause 7.10.3 says welds that fail the acceptance criteria are repaired. With the Engineer's approval, the flaw sizing methods and acceptance criteria of Annex H may be used instead. The commentary's reasoning is that a repair in a highly restrained joint can do more damage than a small, well-characterized flaw.
Annex H requires UT to D1.1 Annex N techniques, by technicians qualified under Annex F who also pass a flaw sizing exam (H3). Its acceptance criteria include:
- Near-surface flaws (H2.1): a flaw at or within 3 mm (1/8 in) of the surface is rejected.
- Embedded flaw height (H2.2): rejected if taller than 6 mm (1/4 in).
- Flaws at backing (H2.3): with backing left in place, a flaw that extends more than 3 mm into the groove weld thickness is rejected.
- Embedded flaw area (H2.4): a single flaw is rejected if its height times length exceeds the square of the effective throat; flaws in any 300 mm (12 in) length are rejected if their total area exceeds 10% of the throat times the weld length.
- Interaction (H2.5, H2.6): aligned or parallel flaws closer than half their combined length or height are treated as one.
MT the D1.8 way: Annex G
Clause 7.9 requires MT to use the yoke method under a written procedure meeting Annex G. Annex G tightens normal practice so that surface cracks and incomplete fusion are reliably found:
- Written procedure (G1) covering weld type, equipment and current, surface preparation, sequence, magnetization plan, particles, interpretation, acceptance and reporting.
- Visual inspection first (G2) and a clean, dry surface (G3).
- Continuous method (G4) with an AC or DC electromagnetic yoke and dry particles visible in white light.
- Articulating-leg yoke (G5); fixed-leg yokes are not allowed. Lifting force at least 4.5 kg (10 lb) for AC and 18 kg (40 lb) for DC at maximum leg spacing, checked and recorded every day (G8).
- Particles used once (G7).
- Yoke placement (G9). For longitudinal flaws, the yoke straddles the weld, stepped no more than half the leg spacing or 75 mm (3 in), whichever is smaller. For transverse flaws, the legs run parallel to the weld about 12 mm (1/2 in) from the toe. Coverage must be 100%, or the report must say what was missed.
- Verifying indications (G11) by retesting at right angles, retesting after removing excess particles and lightly grinding doubtful ones.
- Acceptance (G12). Any relevant indication confirmed as a crack or incomplete fusion is rejected, regardless of length.
MT appears throughout D1.8: after repair welds, at k-area welds, at repaired weld tab sites and on access hole cut surfaces. Our articles on seismic base metal repair and k-area cracking show where.
Shop welds and field welds
UT and MT follow the weld. Demand Critical welds made in the shop, such as column tree flange welds, continuity plates and built-up member welds, are tested at the plant before the steel is coated and shipped, where the access is easiest and a repair costs least. Field-welded beam-to-column connections are tested on site after the erector completes them, which is the US contractor's scope. Agreeing early which welds are shop welds and which are field welds tells the QA agency where its UT technicians need to be and when.
How World Steel supports UT and MT
World Steel schedules UT and MT of Demand Critical welds at our weld inspection and NDT checkpoint, as agreed in the inspection and test plan for each project. Shop NDT is carried out by qualified technicians to written procedures, and the QA agency or a laboratory the customer names can perform or witness the D1.8 testing. Our shop welding procedures and welders are qualified to AWS D1.8, and every NDT report is linked to its piece mark and welder in our IAS AC472-accredited quality system, where the special inspector can review it through inspector access.
For the full picture of who inspects what, read our article on seismic weld QC and QA.
Quick answers
What UT procedure does AWS D1.8 require?
The procedures of AWS D1.1 Clause 8 Part F, following a written procedure with the elements of D1.1 Annex N, qualified on weld mockups with 1.5 mm side drilled holes. Acceptance is to D1.1 Table 8.2.
What is the Annex F test?
A practical exam for UT technicians on mockup welds containing at least 20 known flaws. To pass, a technician needs an overall rating of at least 0.90, a detection rate of at least 0.87 and a false call rate no higher than 0.15.
Can a weld that fails UT be accepted?
With the Engineer's approval, the flaw sizing methods and acceptance criteria of Annex H may be used instead of repair. Near-surface flaws are always rejected.
What MT method does AWS D1.8 require?
The yoke method with dry, visible particles, an articulating-leg yoke and a written procedure to Annex G. Any relevant indication shown to be a crack or incomplete fusion is rejected, whatever its length.
Keep building your steel plan
Go further on USPEB.com
On this topic
Across the US market
- Quality hubInspection, testing and sign-off at the plant
- IAS AC472 accreditationThe first and only AC472 plant in Vietnam
- Online factory auditWalk the shop live with our QA team
- Large projects, 2,500 t a monthCapacity for large US general contractors
- Contractor partnershipLong-term supply for US contractors
- Solutions by stateState-by-state steel solutions