Seismic filler metal toughness: the two CVN tests behind every AWS D1.8 weld

AWS D1.8 asks for weld metal that stays tough when the steel around it yields. It does that with two Charpy tests, a hydrogen limit and a short list of exempt electrodes. Here is how the numbers fit together.

· 7 min read · World Steel USA engineering team

A seismic frame is designed so that the steel yields and the welds do not. That only works if the weld metal is tough enough to tolerate a small flaw, a sharp root or a cold morning while the beam next to it stretches. AWS D1.8 controls this with clear numbers for seismic filler metal toughness, set out in Clause 6.1 and Tables 6.1 to 6.4. This article explains each number, where it comes from and how a fabricator proves it.

Two kinds of weld, two levels of proof

D1.8 recognizes two kinds of weld in the seismic force-resisting system (SFRS):

  • All welds covered by the code. They must meet Part A of Clause 6: strength, elongation, classification toughness and hydrogen.
  • Demand Critical welds. They must also meet Part B: toughness proven across a heat input range, production lot control and FCAW exposure limits.

The split comes from the post-Northridge research. FEMA 267 first asked for 27 J at -18 °C on critical joints. FEMA 353 extended that to all SFRS welds and added 54 J at 21 °C, tested with a heat input procedure. AISC 341 took the same two-level idea and named the second level Demand Critical. D1.8 settled on the test temperatures and kept them consistent with service conditions.

Layer one: Table 6.1 for every SFRS weld

Every filler metal used on welds covered by D1.8 must meet Table 6.1, tested to its AWS A5 specification:

Property 70 ksi class 80 ksi class 90 ksi class
Yield strength, min. 400 MPa (58 ksi) 470 MPa (68 ksi) 540 MPa (78 ksi)
Tensile strength, min. 490 MPa (70 ksi) 550 MPa (80 ksi) 620 MPa (90 ksi)
Elongation, min. 22% 19% 17%
CVN toughness, min. 27 J at -18 °C (20 ft·lbf at 0 °F) 27 J at -18 °C 34 J at -29 °C (25 ft·lbf at -20 °F)

Three notes from the commentary are useful:

  • No maximum strength. Welds are not meant to join in the inelastic mechanism, so over-matching weld metal does not hurt ductility.
  • Colder is fine. A filler metal classified at a colder temperature, such as -29 °C or -40 °C, meets the requirement, because that test is more demanding.
  • The 90 ksi class is for 490 MPa steel. It was added in 2016 so that 70 ksi yield steels accepted by AISC 341 have matching filler metal, with a tougher classification target.

Clause 6.1.3 makes life simpler: the manufacturer's normal Certificate of Conformance is enough proof for Table 6.1 and for hydrogen. The code does not ask the shop to test filler metal samples or production welds for these properties.

Hydrogen: the H16 ceiling

Clause 6.1.2 and Table 6.2 limit diffusible hydrogen. In practice, every electrode or electrode-flux combination must deposit weld metal at H16 or better, which means no more than 16 ml of hydrogen per 100 g of weld metal.

How this is shown depends on the process:

Process How hydrogen is shown
SMAW, carbon and low-alloy Moisture content per the A5.1 or A5.5 specification, or an H16 test per AWS A4.3 at the shop's choice
GMAW, solid wire Exempt from measurement
GMAW, metal-cored wire H16 per AWS A4.3
FCAW, carbon and low-alloy H16 per A5.20 or A5.29
SAW, each wire-flux combination H16 per AWS A4.3
ESW and EGW with composite electrodes As agreed between the Contractor and the Engineer

The commentary's advice is practical: ask the electrode and flux manufacturer for the data up front, because testing after the fact is costly and slows the job. Keeping the low hydrogen level in production is another matter, covered in our article on FCAW electrode exposure limits.

Layer two: Table 6.3 for demand critical welds

For Demand Critical welds made with prequalified WPSs, the filler metal must also meet Table 6.3, proven by the heat input envelope test in Annex A:

Property 70 ksi class 80 ksi class 90 ksi class
Yield, tensile, elongation Same as Table 6.1 Same as Table 6.1 Same as Table 6.1
CVN toughness, min. 54 J at 21 °C (40 ft·lbf at 70 °F) 54 J at 21 °C 54 J at 10 °C (40 ft·lbf at 50 °F)

The 54 J level and the 21 °C test temperature come from the SAC research, and they suit enclosed buildings. The important difference from Table 6.1 is how the test is made. Annex A welds two test plates, one at a low heat input and one at a high heat input, and takes five Charpy specimens and a tensile specimen from the middle of each. The highest and lowest Charpy results are dropped; two of the remaining three must reach 54 J and the third may be no lower than 40 J, with the average at least 54 J. Toughness tends to fall at both extremes of heat input, so passing both plates shows the filler metal stays tough anywhere between them.

For WPSs qualified by test, the PQR itself must meet Table 6.3 (Clause 6.2.4), so Annex A is not needed. See our article on heat input envelope testing.

Electrodes that skip the envelope test

Some filler metals reliably deposit tough weld metal. Table 6.4 lists classifications that are exempt from Annex A testing when the Lowest Anticipated Service Temperature is 10 °C (50 °F) or warmer:

  • SMAW: E7018, E7018-1, E7018-C3L and E8018-C3
  • GMAW solid wire: ER70S-2, -3, -6, -7 and -8, and ER80S-Ni types

These same products can also be exempt from production lot testing under Clause 6.3.4 when they show at least 27 J at -18 °C on the certificate. Flux cored wires and submerged arc combinations are not on the list, so they need envelope data from the manufacturer or from the fabricator's own testing.

When the building is cold

Many seismic buildings are heated offices or warehouses. Others are not: parking structures, canopies, pipe racks, cold storage and buildings in Alaska or the mountain West. When the SFRS will see service temperatures below 10 °C, the Engineer sets the Lowest Anticipated Service Temperature (LAST), and Clause 6.2.2 moves the Demand Critical test temperature:

  • 70 and 80 ksi filler metals: test at no more than 11 °C (20 °F) above LAST
  • 90 ksi filler metals: test at LAST

The Table 6.4 exemptions stop applying below 10 °C. Our article on lowest anticipated service temperature works through examples.

Mixing processes in one joint

One more toughness trap sits in Clause 6.1.4. When self-shielded flux cored wire (FCAW-S) is combined in the same joint with another process, such as a gas-shielded root and a self-shielded fill, the mixed weld metal can lose toughness even though each product passes on its own. D1.8 then requires the Annex B intermix test. It matters most where shop and field welding meet, and is covered in our article on FCAW-S intermix testing.

What about the steel and the heat-affected zone?

D1.8 controls the weld metal. Base metal toughness comes from AISC 341 and the ASTM specification, normally shown on mill test certificates with Charpy results where required, as explained in our article on steel mill test certificates. The commentary notes that the heat-affected zone also matters, especially above about 3.1 kJ/mm (80 kJ/in) heat input, which is uncommon with SMAW, FCAW and single-wire SAW but common with multi-wire SAW and electroslag welding. At those heat inputs, the Engineer may ask for extra HAZ testing.

A shop routine for filler metal approval

Turning these tables into daily practice takes a short, repeatable routine. Ours runs in five steps for each filler metal on a seismic job:

  1. Identify the weld category. From the weld map, list which joints are SFRS welds and which are Demand Critical, and the LAST that applies.
  2. Match the classification. Confirm the AWS classification meets Table 6.1, including the toughness temperature, and for 490 MPa steel that the 90 ksi class is used where the design needs it.
  3. Check the second layer. For Demand Critical welds, confirm the product is on Table 6.4 and LAST is 10 °C or warmer, or collect Annex A envelope data for the exact trade name and diameter.
  4. Check hydrogen and storage. File the H16 evidence, and for FCAW the manufacturer's exposure guidance or Annex E data.
  5. Lock it into the WPS. Write the manufacturer and trade name into the WPS, set the heat input range inside the tested envelope, and release the product to the floor only for the joints it is approved for.

Most of the toughness problems found on seismic jobs trace back to skipping one of these steps, usually step 3 when a new brand of flux cored wire arrives.

What inspectors usually ask

Special inspectors and QA agencies tend to ask the same questions about filler metal on seismic work. Is the product on the WPS the one on the feeder? Is the certificate for this classification and diameter? Where is the envelope data or the Table 6.4 exemption? Is the exposure log current? Having the answers in one folder per WPS makes an inspection short.

How World Steel proves weld metal toughness

At World Steel, each filler metal for a seismic job is checked against Table 6.1 and, for Demand Critical welds, Table 6.3 or Table 6.4 before it is issued to the floor. Certificates of Conformance, hydrogen data and envelope data are filed against the WPS and the project. Plate for seismic members can be supplied with EN 10204 3.1 certificates including Charpy results on request, and any confirmation testing is done at an ISO/IEC 17025 laboratory or one the customer names. Our shop welding procedures and welders are qualified to AWS D1.8, and our quality system is accredited to IAS AC472.

For the wider picture of seismic material requirements, see our page on seismic steel toughness and mill certificates.

Quick answers

What CVN toughness does AWS D1.8 require for all SFRS welds?

For 70 and 80 ksi filler metals, 27 J (20 ft·lbf) at -18 °C (0 °F) in the AWS classification test. For 90 ksi filler metals, 34 J (25 ft·lbf) at -29 °C (-20 °F).

What extra toughness do demand critical welds need?

At least 54 J (40 ft·lbf) at 21 °C (70 °F) for 70 and 80 ksi classes, or at 10 °C (50 °F) for 90 ksi, in welds made at both a high and a low heat input. Colder service temperatures lower the test temperature.

Is there a maximum weld metal strength?

No. Table 6.1 values are minimums. Welds are not meant to yield in a seismic frame, so higher weld metal strength does not reduce the frame ductility.

What hydrogen level is allowed?

Diffusible hydrogen of H16 or lower, meaning no more than 16 ml per 100 g of deposited weld metal, shown by the manufacturer certificate or by moisture content for SMAW electrodes.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

AWS D1.8 seismic fabrication series

Twenty in-depth articles that follow a seismic weld from the drawings to the last test report. Each one explains a part of AWS D1.8:2025 in plain terms and lists the checks a general contractor can ask the fabricator about.

Drawings and scope

What the code covers, which welds are Demand Critical, and the data the drawings must carry.

Procedures and welders

The WPS, the restricted access welder test and the bottom flange sequence.

Details and Protected Zones

Access holes, backing, weld tabs, k-area details, Protected Zones and repairs.

Inspection and testing

Who inspects what, inspector qualifications, and UT and MT done the D1.8 way.

Bidding a large US project?