Skip to content
Seeking US contractor partners IAS AC472 ACCREDITED ★ METAL BUILDINGS ★ AC472 IAS AC472 accreditedIAS AC472
World Steel USA
Fabricated steel members lining a covered aisle in the World Steel plant

Quality and certification

FCAW electrode exposure limits: moisture control for seismic welds

Flux cored wire can soak up moisture from humid air, and moisture means hydrogen in the weld. AWS D1.8 caps how long FCAW wire may sit exposed before it is used on a demand critical weld. Here is the rule and how a shop keeps track.

· 7 min read · World Steel USA engineering team

Flux cored arc welding (FCAW) is the workhorse process for structural steel. It deposits metal fast, works in all positions and suits both shop and field. But the flux inside the tubular wire can absorb moisture from the air, and moisture breaks down in the arc into hydrogen that dissolves in the weld. Hydrogen raises the risk of cracking, sometimes hours after welding. For the welds a seismic frame depends on, AWS D1.8 Clause 6.4 adds strict FCAW electrode exposure limits. This article explains them, what the Annex E test proves, and how a shop can keep an honest record of every spool.

Why the code singles out FCAW

The commentary sets out the reasoning. FCAW electrodes, like covered SMAW electrodes, can absorb moisture, and the rate depends on the design of the product. Because SFRS welds are critical and an undetected crack could matter in a major earthquake, D1.8 imposes extra exposure controls on FCAW. For SMAW electrodes, the existing D1.1 rules on storage, exposure and baking are considered enough. Solid GMAW and SAW wires carry no flux inside, so they have no exposure limits beyond being kept clean and dry, though SAW flux has its own storage needs.

These rules apply to Demand Critical welds only. Other SFRS welds still need filler metal that meets the H16 hydrogen limit of Clause 6.1.2, but without the exposure clock.

Hydrogen cracking in brief

Hydrogen-assisted cracking, often called cold cracking or delayed cracking, needs three things at the same time: hydrogen in the weld or heat-affected zone, a hard and susceptible microstructure, and tensile stress, including the residual stress left by welding. Seismic joints tend to bring the last two. Thick column flanges cool welds quickly, and heavily restrained beam-to-column joints carry high residual stress. That leaves hydrogen as the factor the shop can control most directly.

Hydrogen control works in layers. The filler metal must be designed and certified for low hydrogen, which is the H16 limit of Clause 6.1.2. Preheat, set by AWS D1.1 for the steel and thickness, slows cooling and lets hydrogen diffuse out. Clean, dry joints remove other sources, such as rust, oil and condensation. Exposure limits protect the first layer: a wire certified at H16 in the factory can drift above it after days in humid air.

These cracks can appear hours or even days after welding, which is one reason inspection timing matters. AWS D1.8 itself recognizes delayed cracking in the k-area, where MT is not done until at least 48 hours after welding. A crack that forms after the inspector leaves is the hardest kind to catch, so prevention at the wire is far cheaper than detection later.

Packaging: the first line of defense

Clause 6.4.1 requires FCAW electrodes to come in protective packaging that limits moisture pickup. When taken out of the package, the wire must still be able to deposit weld metal within the H16 hydrogen limit.

The commentary points out that packaging ranges from plain cardboard boxes to hermetically sealed foil bags, and not all of it protects the wire. Opened or damaged packaging protects nothing. So:

  • Wire from a punctured or torn package may not be used on Demand Critical welds unless it has been dried to the manufacturer's recommendations.
  • Clause 6.4.2 forbids modifying or lubricating the electrode after manufacture, apart from manufacturer-approved drying.

The exposure clock

Clause 6.4.3 sets the permissible accumulated exposure time after the wire leaves its protective packaging. There are three tiers:

Tier Basis for the limit Exposure allowed
1 Manufacturer's guideline, based on exposure tests to Annex E As stated by the manufacturer
2 The shop's own Annex E test of the product As shown by the test
3 No Annex E data available 72 hours accumulated

Two details matter in practice:

  • The clock is cumulative. Two days on the feeder, a week in a cabinet, then another day on the feeder counts as three days, not one.
  • Protected storage stops the clock. Time in protective packaging or a storage cabinet is not counted. The commentary explains that when welding is suspended, wire can be stored where it gains no more moisture, and the clock resumes when it is put back on the machine.

The commentary also notes that test data suggests 72 hours is a conservative upper limit when no product-specific data exists.

What Annex E tests

Annex E is how a manufacturer, or a fabricator, earns a longer exposure limit than 72 hours. The method:

  • Exposure. The wire sits in an environmental chamber at 27 °C (+3/-0 °C) and 80% (+5/-0%) relative humidity for the full exposure period to be approved. Time, temperature and humidity are recorded continuously.
  • No reconditioning. After exposure, the wire is welded as it is, with no drying.
  • Hydrogen test. Diffusible hydrogen is measured by the AWS A5.20 method, either with the production diameter or with one diameter larger and one smaller.
  • Acceptance. The exposure period is approved if the weld metal stays at H16 or lower, meaning no more than 16 ml of hydrogen per 100 g of weld metal.

Based on the results, the manufacturer, or a consultant approved by the Engineer, gives storage and exposure recommendations. These may be a fixed period, or limits that vary with temperature and humidity. They may also include heated storage or baking, but rebaking is only allowed when the manufacturer approves it and tests show the wire returns to H16 or better afterwards.

The 27 °C and 80% humidity condition is worth noticing. It is a deliberately humid environment, close to normal everyday conditions in Southeast Asian shops and the US Gulf Coast in summer. A product approved at that condition behaves predictably in real shops.

Overexposed wire

Clause 6.4.4 gives two choices for wire that has exceeded its limit:

  1. Dry it to the manufacturer's recommendations, which must state the time, the temperature and how many drying cycles are permitted. Some products are not meant to be dried at all.
  2. Move it to work other than Demand Critical welds.

If a spool goes through more than one cycle of exposure and drying, the manufacturer's guidance must say that is allowed.

Keeping an honest exposure log

The rule is simple. The record-keeping is where shops slip. A practical system includes:

  • A tag on every spool opened for Demand Critical work, showing the trade name, diameter, lot, opening date and time, and the approved exposure limit.
  • Log entries each time the spool moves between feeder and cabinet, so accumulated exposure can be added up.
  • Dedicated storage, such as sealed cabinets or heated stores where the manufacturer recommends them, close to the welding stations so returning wire is easy.
  • A simple end-of-shift rule, for example that partly used spools on Demand Critical work go back into storage at the end of each shift.
  • Visual cues, such as color tags, that separate Demand Critical wire from general-purpose wire.
  • Records kept with the job. Clause 1.4.2.5 requires the Annex E documentation to be kept when exposure limits are extended.

Weather, climate and field welding

Exposure limits are written around the wire, but climate decides how hard they are to meet. In a humid shop, the 72-hour default can pass quickly when a spool is left on a feeder over a weekend. In the field, wire may sit on a machine outdoors through a wet week. Field crews welding Demand Critical joints need the same tags and logs as the shop, and storage that works on a jobsite. That field work, including any FCAW-S wire used by the erector, is the US contractor's scope, and its compatibility with shop welds is covered in our article on FCAW-S intermix testing.

A useful habit for both shop and field is to plan wire quantities by shift. Opening a spool sized for the welds planned that day, rather than a large drum that will sit on the feeder for a week, keeps exposure short and the log simple.

Questions a general contractor can ask

  1. Which FCAW products are used on Demand Critical welds, and what exposure limit applies to each?
  2. Is the limit from manufacturer Annex E data, your own Annex E test, or the 72-hour default?
  3. How do you track accumulated exposure, and can we see a sample log?
  4. What happens to wire that exceeds the limit?
  5. Do the manufacturer's data sheets with storage and exposure guidance come with the WPSs, as Clause 1.4.2.3 requires?

How World Steel controls FCAW exposure

World Steel's plant in Vietnam works in a humid tropical climate, so moisture control on consumables is part of everyday practice, not a special measure. For seismic jobs, FCAW wire approved for Demand Critical welds is stored in protective conditions, tagged when opened, and logged by accumulated exposure against the limit for that product. Data sheets and Annex E documentation sit with the WPS in the project quality file, and exposure records can be reviewed by the QA agency, in person or through remote inspector access. Our shop welding procedures and welders are qualified to AWS D1.8, under a quality system accredited to IAS AC472.

For the related controls on filler metal, read seismic filler metal toughness and filler metal production lot control.

Quick answers

How long can FCAW wire be exposed under AWS D1.8?

For demand critical welds: up to the manufacturer's limit when that limit is based on Annex E testing, or up to a limit set by the shop's own Annex E test, or 72 hours of accumulated exposure when there is no test data.

Does time in a cabinet count as exposure?

No. Time in protective packaging or in a storage cabinet is not counted. The clock restarts when the wire goes back on the feeder.

What happens to overexposed wire?

It must be dried to the manufacturer's instructions, which must state time, temperature and how many drying cycles are allowed, or it must not be used on demand critical welds.

What is the Annex E test?

Wire is held at 27 °C and 80% relative humidity for the exposure period to be approved, then welded without reconditioning and tested for diffusible hydrogen. It must stay at H16 or lower.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

AWS D1.8 seismic fabrication series

Twenty in-depth articles that follow a seismic weld from the drawings to the last test report. Each one explains a part of AWS D1.8:2025 in plain terms and lists the checks a general contractor can ask the fabricator about.

Drawings and scope

What the code covers, which welds are Demand Critical, and the data the drawings must carry.

Procedures and welders

The WPS, the restricted access welder test and the bottom flange sequence.

Details and Protected Zones

Access holes, backing, weld tabs, k-area details, Protected Zones and repairs.

Inspection and testing

Who inspects what, inspector qualifications, and UT and MT done the D1.8 way.

Bidding a large US project?

Send the bid documents, or just a footprint and an address. Our engineers check them against US code requirements and confirm what World Steel would supply, from a plant that fabricates 2,500 metric tons of structural steel a month.