Ask a welding engineer why one seismic weld passes a Charpy test and its twin fails, and the answer is often heat input. The energy put into each pass sets the bead size and the cooling rate, and those set the weld metal's microstructure. AWS D1.8 does not leave that to chance. For Demand Critical welds made with prequalified procedures, it requires heat input envelope testing of the filler metal under Annex A, and then holds production welding inside the envelope that test proved. This article explains why, how the test is run, and what it means on the shop floor.
Why heat input matters for toughness
Heat input is the arc energy delivered per unit length of weld. For a conventional power source, D1.1 and D1.8 compute it as:
Heat input (kJ/mm) = (60 × volts × amps) / (1000 × travel speed in mm/min)
Higher heat input means a bigger bead and a slower cooling rate. Lower heat input means a smaller bead that cools fast. The D1.8 commentary explains the effects:
- Strength and elongation of common E70 and E80 weld metal change only a little across the normal range.
- Charpy toughness changes much more, and it tends to fall at both extremes. Too cold and fast, and the weld can be hard and brittle; too hot and slow, and the grain coarsens.
- Results from welds between the two extremes are usually better than either extreme.
That last point is the logic of the envelope. If a filler metal passes at the lowest and the highest heat input you will use, you can expect it to pass anywhere in between.
When Annex A applies
Clause 6.2.1 requires Annex A testing for filler metals used on Demand Critical welds with prequalified WPSs. It does not apply to:
- welds that are covered by D1.8 but not Demand Critical
- WPSs qualified by test, where the PQR does the same job (Clause 6.2.4)
- filler metals listed in Table 6.4, such as E7018 SMAW electrodes and ER70S solid GMAW wires, as long as the Lowest Anticipated Service Temperature (LAST) is 10 °C (50 °F) or warmer
The test may be run by the filler metal manufacturer, by the fabricator, or by a third party acceptable to the Engineer (Clause 6.2.3). Whoever runs it, the fabricator is responsible for making sure it exists for the exact products on its WPSs, and Clause 1.4.2.2 asks for the certification to be on file.
How the Annex A test works
Annex A is short and specific. In outline:
Two plates. One plate is welded at a computed heat input no lower than the maximum to be used in production. The other is welded at no higher than the minimum to be used in production.
Suggested levels. Table A.1 suggests:
| Test | Suggested heat input | Preheat | Interpass |
|---|---|---|---|
| Low heat input | 1.2 kJ/mm (30 kJ/in) | 49 °C (120 °F) maximum | 121 °C (250 °F) maximum |
| High heat input | 3.1 kJ/mm (80 kJ/in) | 121 °C (250 °F) minimum | 232 °C (450 °F) minimum |
These limits are suggestions. A manufacturer may test a narrower range when a product cannot meet the properties at the extremes, or a wider range when it can. Production then uses whatever range was actually tested.
Control during welding. Each pass must stay within ±20% of the target heat input. Interpass temperature is measured before every pass. For the high heat input plate, the plate is brought to the minimum preheat and welded without deliberate breaks until it reaches the minimum interpass temperature, then held there. The test plates may be preset or restrained to stay within 5° of flat, and a warped plate is discarded, not straightened. No heat treatment is allowed, except a short low-temperature aging of the machined tensile bar.
Base metal. Plates for E70 filler metals are ASTM A36, A572 Grade 50 or A992. Higher-strength filler metals use higher-strength plates from a short list.
Specimens. From each plate: five Charpy V-notch specimens and one all-weld-metal tensile specimen, taken from the weld center at mid-thickness to limit dilution from the base metal.
Acceptance criteria
Each plate must meet Table A.2:
| Property | E70 | E80 | E90 |
|---|---|---|---|
| Yield strength, min. | 400 MPa | 470 MPa | 540 MPa |
| Tensile strength, min. | 490 MPa | 550 MPa | 620 MPa |
| Elongation, min. | 22% | 19% | 17% |
| CVN, LAST 10 °C or warmer | 54 J at 21 °C | 54 J at 21 °C | 54 J at 10 °C |
For the Charpy results, the highest and lowest of the five values are discarded. Of the remaining three, two must be at least 54 J (40 ft·lbf), one may be lower but not below 40 J (30 ft·lbf), and the average of the three must reach 54 J. When the Engineer sets a LAST below 10 °C, the test temperature drops as described in our article on lowest anticipated service temperature.
From test result to WPS limits
Once a filler metal has passed, Clause 6.8.1 says production heat input for prequalified Demand Critical WPSs must stay within the tested range. The commentary spells out what that means in practice:
- The WPS must name the electrode manufacturer and trade name (Clause 6.6.2), because each product has its own envelope.
- The welder does not need to copy the test's volts, amps and travel speed. Any combination is fine as long as the computed heat input falls between the low and high test values.
- If the WPS shows ranges of current, voltage or travel speed, the shop must check that every combination in those ranges still lands inside the envelope.
- Stringer beads and weave beads are both allowed, as long as heat input stays in range. D1.1 limits on layer thickness and bead width still apply.
For WPSs qualified by test, the rule is different (Clause 6.2.4 and 6.8.2). Each fill pass in the qualification test must be within ±10% of the test's average heat input, and production may run from 80% to 120% of that average. The PQR must meet Table 6.3. The commentary notes these are the same limits used in AASHTO/AWS D1.5 for bridge work.
A worked example
Suppose a flux cored wire has been tested by its manufacturer at 1.2 kJ/mm and 3.1 kJ/mm and passed both. A fabricator writes a prequalified WPS for beam flange welds with 260 A, 26 V and a travel speed between 250 and 400 mm/min.
- At 400 mm/min: 60 × 26 × 260 / (1000 × 400) ≈ 1.01 kJ/mm, below the tested minimum.
- At 250 mm/min: 60 × 26 × 260 / (1000 × 250) ≈ 1.62 kJ/mm, inside the envelope.
The WPS has to narrow the travel speed range, for example to 250 to 330 mm/min, which gives about 1.62 down to 1.23 kJ/mm. The example is illustrative; real limits come from the manufacturer's data and the shop's own checks.
Heat input, preheat and interpass: three separate controls
It is easy to blur three controls that D1.8 keeps apart. Heat input is set by the welding parameters and checked against the envelope. Preheat and minimum interpass temperature protect against hydrogen cracking and follow AWS D1.1 for the steel grade and thickness, measured at least 75 mm (3 in) from the joint so the whole volume around the weld is warm enough. Maximum interpass temperature protects toughness from slow cooling and is capped by Clause 6.7 at 288 °C (550 °F), measured 25 to 75 mm (1 to 3 in) from the joint.
The temperatures in Table A.1 belong to the test only. The commentary is explicit that production preheat and interpass controls come from D1.1 and D1.8, and will usually differ from the Annex A test plate limits. A shop that copies the Annex A preheat into its WPS has misunderstood the test.
On thick seismic members the three controls interact. A heavy column flange needs high preheat, and repeated passes in a confined groove can push the interpass temperature toward the 288 °C ceiling. Welders then have to pause between passes while still keeping the minimum interpass temperature, which is why interpass checks with contact thermometers or temperature crayons, placed outside the joint area, are part of every Demand Critical weld record in a well-run shop.
Heat input and the heat-affected zone
D1.8 does not require heat-affected zone (HAZ) toughness testing, but the commentary is clear that HAZ toughness still matters. Studies cited there show HAZ transition temperature tends to rise with heat input, and that heat inputs of about 1.2 to 2.8 kJ/mm should not seriously harm HAZ toughness in common structural steels. SMAW, FCAW, GMAW and single-wire SAW rarely exceed 3.1 kJ/mm. Multi-wire SAW and electroslag welding often do, and at those levels the Engineer may want extra testing of the steel's HAZ.
Common mistakes
- Using one brand's envelope data for another brand of the same AWS class.
- Writing wide WPS ranges that let a welder drift outside the envelope.
- Ignoring waveform-controlled machines, where heat input is computed from instantaneous power or energy rather than the simple formula.
- Assuming the exemption of Table 6.4 on an open structure where LAST is below 10 °C.
How World Steel works inside the envelope
At World Steel, every Demand Critical WPS names its filler metal by manufacturer and trade name and carries a heat input table checked against the envelope data on file. Welding parameters are set on the machines to keep the computed heat input in range, and our QC inspectors check amperage, voltage and travel speed on Demand Critical joints during production. The WPSs, envelope certificates and parameter checks go into the project quality file under our IAS AC472-accredited system.
For how the WPS ties all of this together, read our article on seismic WPS requirements, and for the other filler metal controls see seismic filler metal toughness.
Quick answers
What is heat input envelope testing?
An AWS D1.8 Annex A test in which a filler metal is welded on two plates, one at a high heat input and one at a low heat input, and each weld must meet the demand critical strength and toughness values. Production welds made between the two heat inputs are then accepted.
What heat inputs does Annex A suggest?
About 1.2 kJ/mm (30 kJ/in) for the low test and 3.1 kJ/mm (80 kJ/in) for the high test. These are suggestions; a narrower or wider range can be tested and then used.
Who does the test?
The filler metal manufacturer, the fabricator or a third party acceptable to the Engineer. The fabricator stays responsible for making sure it has been done.
What if the WPS is qualified by test?
Annex A is not needed. Heat input must stay within 80% to 120% of the average heat input of the qualification test, and that test must meet the demand critical properties.
Keep building your steel plan
Go further on USPEB.com
On this topic
Across the US market
- US codes and standardsIBC, AISC, AWS and MBMA, designed to
- Seismic steel structuresSDC D to F framing for West Coast jobs
- Crane building designUS crane standards for mill and bay buildings
- Design ReportWhat our US-code design report contains
- Large projects, 2,500 t a monthCapacity for large US general contractors