Stiffened steel members with end plates lined up in the World Steel plant

Engineering and codes

Bottom flange weld sequence: how seismic beam-to-column welds are laid down

The worst defects found after Northridge sat under the beam web, where weld passes started and stopped. AWS D1.8 Clause 6.9 fixes that with a simple sequence for bottom flange welds. Here is the rule, the reasoning and the shop practice.

· 7 min read · World Steel USA engineering team

Some code rules take pages. Clause 6.9 of AWS D1.8 takes three lines, and it may prevent more fractures than any other. It sets the bottom flange weld sequence for complete joint penetration (CJP) groove welds that join a beam bottom flange to a column flange, or to a continuity plate, when the weld has to be made through a weld access hole. This article explains the rule, the evidence behind it and how a shop puts it into practice, together with the welder identification rule of Clause 6.10 that makes the sequence traceable.

The problem under the web

On a welded beam-to-column moment connection, the beam's top flange can be welded from above with nothing in the way. The bottom flange is different. The beam web sits on top of the bottom flange, right in the middle of the joint, so the welder has to work through an access hole cut in the web, reaching around the web to weld the part of the groove beneath it.

The D1.8 commentary records what investigators found after the 1994 Northridge earthquake: incomplete fusion and entrapped slag under the beam web, against the column face. The pattern suggested that weld passes were being started or stopped at that one spot, layer after layer. Weld starts and stops are where defects are most likely: the arc has not yet stabilized at a start, and a crater forms at a stop. When every layer begins or ends at the same place, the defects stack up into one large flaw at the point of highest stress.

Why this matters more than it looks

It is tempting to treat Clause 6.9 as a small workmanship note. The research says otherwise. Under earthquake loading the bottom flange weld of a moment connection carries the full tension of the beam flange as the beam yields and strain hardens nearby. The highest stress is at the root, right at the column face, in the middle of the flange width, which is exactly the zone under the web. A flaw only a few millimetres tall in that spot acts like a pre-cut crack. The Northridge connections that fractured often did so at loads well below what the beams could carry, because a crack started at such a flaw and ran across the flange or into the column.

Moving the starts and stops costs almost nothing: a few seconds of planning per layer and some discipline. Finding and repairing a stacked defect under the web after the joint is finished costs gouging, rewelding, preheating, MT and a repeat UT, all in the most restrained part of the connection. That balance is why inspectors watch this sequence closely on Demand Critical joints.

The rule

Clause 6.9 applies to CJP groove welds of beam bottom flanges to column flanges, or of beam bottom flanges to continuity plates, made using weld access holes. They are sequenced so that:

  1. As far as practicable, starts and stops are not directly under the beam web.
  2. Each layer is completed across the full width of the flange before the next layer begins.
  3. For each layer, the starts and stops are on the opposite side of the beam web from those of the previous layer.

The commentary adds two points. Staggering starts and stops on alternate sides of the web reduces the problem provided proper cleaning is done after each pass. And the direction of travel is not controlled by the rule: a welder may travel left to right or right to left, as long as the starts and stops land where the rule puts them.

What the sequence looks like

Picture the bottom flange from above, with the beam web running along the beam's length in the middle of the flange width:

Layer Pass start and stop location Note
Root Begins on the weld tab on one side, runs through the zone under the web, ends on the opposite tab The pass runs continuously under the web
Second layer Starts and stops on the opposite side of the web from the root's Full width before moving on
Third layer Back to the first side Alternating continues
Fill and cap Keep alternating side to side Each layer complete across the width

In practice a welder often has to stop partway, for example to reposition around the web. The rule then asks that the stop is not directly under the web, that the next start overlaps properly after the crater is cleaned, and that the following layer moves its start and stop to the other side. Weld tabs, extending at least 25 mm or the flange thickness beyond each edge (Clause 6.16.1), let the welder start and stop outside the joint at the flange edges.

Cleaning between passes

The commentary's condition, proper cleaning after each pass, is half the rule. Slag trapped in a corner under the web becomes a slag inclusion in the next layer. Good practice for these joints includes:

  • removing slag fully after every pass, with particular attention to the toes along the column face and under the web
  • grinding out start and stop craters before overlapping them
  • checking interpass temperature before each pass (maximum 288 °C, measured 25 to 75 mm from the joint, Clause 6.7)
  • visual inspection of each layer by the welder and spot checks by QC, before the zone under the web is covered

Who welds these joints

The same joint is the one that triggers the restricted access welder test of Annex D. A welder making a Demand Critical bottom flange CJP weld through an access hole must have passed it, in the production process, with the production backing type and at a deposition rate at least as high as production. Our article on the restricted access welder test explains it.

After the weld: backing, root and fillet

Clause 6.9 governs the groove weld. What happens next depends on the connection and the contract documents:

  • On many prequalified moment connections, steel backing at the bottom flange is removed, the root is backgouged to sound metal and back welded, and a reinforcing fillet of at least 8 mm (5/16 in) is added at the column face (Clauses 6.13 and 6.14).
  • Weld tabs at the flange edges are removed and the ends finished smooth (Clause 6.16.3).
  • The bottom flange is the joint where Northridge showed left-in-place backing was most harmful, because the unfused edge of the backing sits at the point of highest stress.

Our articles on weld backing removal and weld tab removal cover those steps.

Welder identification

Clause 6.10 requires the contractor to have a system that identifies the welder or welders who welded each joint. The commentary gives two reasons:

  1. It helps find the source of consistently poor welds, so a problem welder or technique can be corrected.
  2. It can support a reduction in NDT for highly qualified welders with consistent quality, under the rules of the QAP.

If stamps are used, they must be low-stress types, with rounded characters, so they do not create sharp notches near the joint that could start a crack when the steel yields. Many shops now use paint markers, tags or digital records linked to piece marks instead of stamps on the steel.

Where the sequence applies in a frame

The bottom flange sequence is most often met in:

  • Special and intermediate moment frames with welded flange connections, such as welded unreinforced flange-welded web (WUF-W) connections and reduced beam section (RBS) connections with CJP flange welds, both prequalified in AISC 358.
  • Shop-welded column trees, where beam stubs are welded to columns in the shop and spliced to the beams in the field.
  • Beam-to-continuity plate welds, where the beam frames into a column through continuity plates and the bottom flange joint is welded through an access hole.

Field-welded moment connections, the most common US case, are welded by the erector, which is the US contractor's scope. Shop-welded column trees and prefabricated moment frame modules are welded by the fabricator.

Checklist for the bottom flange joint

  1. Welder holds D1.1 qualification and the Annex D restricted access qualification for the process and backing.
  2. Weld tabs fitted, at least 25 mm or flange thickness long, tacked inside the joint where in a Protected Zone.
  3. Access hole geometry as specified, with cut surfaces smooth and checked.
  4. Starts and stops not under the web; each layer full width; sides alternate layer by layer.
  5. Slag cleaned and craters ground after every pass.
  6. Interpass temperature checked against the 288 °C maximum and the WPS minimum.
  7. Welder identification recorded for the joint.
  8. Backing, root and tab treatment as the contract documents require, followed by the specified NDT.

How World Steel applies the sequence

World Steel fabricates column trees, moment frame members and built-up columns such as welded box columns for seismic projects in the United States. On shop-welded bottom flange joints made through an access hole, the Clause 6.9 sequence is written into the work instruction for the joint, and our welders mark the joint with their identification. Our shop welding procedures and welders are qualified to AWS D1.8, and every Demand Critical joint is recorded in our IAS AC472-accredited quality system with its welder, filler metal and inspection result.

Where the moment connections are field welded, our shop drawings show the access hole geometry, backing and weld tab details so the erector's crew can follow the same sequence on site.

Quick answers

What does AWS D1.8 Clause 6.9 require?

For CJP welds of beam bottom flanges to column flanges or continuity plates made through an access hole: avoid starts and stops under the beam web where practicable, finish each layer across the full flange width, and put each layer's starts and stops on the opposite side of the web from the layer before.

Does it control the direction of travel?

No. The commentary says the direction of weld travel is not controlled by this provision.

Why does welder identification matter?

It traces poor-quality joints back to their source, and it can support reduced NDT for welders with a consistent record. Stamps, if used, must be low-stress to avoid notches.

Does the sequence apply to the top flange?

Clause 6.9 is written for bottom flange welds made through a weld access hole. Top flange welds follow the general D1.1 and D1.8 rules.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

AWS D1.8 seismic fabrication series

Twenty in-depth articles that follow a seismic weld from the drawings to the last test report. Each one explains a part of AWS D1.8:2025 in plain terms and lists the checks a general contractor can ask the fabricator about.

Drawings and scope

What the code covers, which welds are Demand Critical, and the data the drawings must carry.

Procedures and welders

The WPS, the restricted access welder test and the bottom flange sequence.

Details and Protected Zones

Access holes, backing, weld tabs, k-area details, Protected Zones and repairs.

Inspection and testing

Who inspects what, inspector qualifications, and UT and MT done the D1.8 way.

Bidding a large US project?