Skip to content
Seeking US contractor partners IAS AC472 ACCREDITED ★ METAL BUILDINGS ★ AC472 IAS AC472 accreditedIAS AC472
World Steel USA
Welded steel base plates and stiffeners lined up for inspection at the World Steel plant

Engineering and codes

Weld tab removal and end dams on seismic groove welds

Weld tabs let a welder start and stop a groove weld outside the joint, where defects do no harm. In a seismic frame they usually have to come off afterwards, and how they come off matters. Here is what AWS D1.8 asks.

· 8 min read · World Steel USA engineering team

Every groove weld has two ends, and the ends are where welds go wrong. When the arc starts, it has not yet settled into the joint and fusion can be poor. When the arc stops, it leaves a crater that can shrink and crack. A weld tab, sometimes called a runoff tab or extension bar, is a short piece of steel placed at the end of a groove so the welder can start and stop beyond the joint, leaving the defects on a piece that does not carry load. In a seismic frame those tabs usually have to come off when the weld is finished. AWS D1.8 Clauses 6.16 and 6.17 set the rules for tab length, tack welds, weld tab removal and the end dams that sometimes sit at the ends of tabs. This article goes through each rule and the reasons behind it.

Why weld tabs are used at all

A complete joint penetration (CJP) groove weld is meant to be full size from one edge of the flange to the other. Without tabs, the welder has to start and stop right at the edge, and the weld ends up undersized, with a crater and poor fusion at the very corner of the flange. That corner is where a beam flange carries some of its highest strains when the frame yields in an earthquake.

Tabs extend the groove past the edge. The welder starts on the tab, travels across the full joint, and stops on the opposite tab, so every pass is sound and full size across the real joint width. The defects stay on the tabs. The bottom flange sequence of Clause 6.9 relies on the same idea: tabs at both flange edges give the welder somewhere to start and stop that is not under the beam web. Our article on the bottom flange weld sequence explains how the two work together.

How long a weld tab must be

Clause 6.16.1 sets the length. Where practicable, a weld tab must extend beyond the edge of the joint by at least:

  • 25 mm (1 in), or
  • the thickness of the part,

whichever is greater. The tab need not be longer than 50 mm (2 in).

Where there is not enough room for tabs, for example where pieces are closely spaced or meet at acute angles, the weld ends may be cascaded for about one weld size instead. The commentary gives the typical cases: joints shown welded full length into pieces with small clipped corners, and the corners of continuity plates next to the k-area of columns, where the full tab length is simply not available.

Tack welds that hold weld tabs

In a Protected Zone, Clause 6.16.2 requires the tack welds that attach weld tabs to be made inside the joint, meeting the general tack weld rules of Clause 6.12. The commentary explains why: a tack weld outside the joint can leave a notch or a small hard spot that becomes a crack starter when the steel yields. A tack weld inside the joint is consumed by the passes that follow and its heat-affected zone is tempered, so it becomes part of the final weld.

If a tack weld is misplaced in the Protected Zone, Clause 6.12.4 requires it to be removed by grinding, and gouges or notches repaired regardless of size, either by grinding under Clause 6.19.1 or by welding under Clause 6.19.2. Our article on protected zone fabrication rules covers the other limits that apply there.

Weld tab removal step by step

When the contract documents require tabs to be removed, Clause 6.16.3 sets the method and the finish:

  1. Remove the tab. Use air carbon arc gouging, grinding, chipping or thermal cutting, and control the process to minimize errant gouging into the finished weld or the base metal.
  2. Finish the weld end. The edge where the tab was must have a surface roughness of no more than 13 µm (500 µin). AWS C4.1 sample 4 may be used as a guide for judging it.
  3. Shape the contour. Grinding flush is not required, but the weld end must give a smooth transition, free of notches and sharp corners. At T-joints a minimum corner radius is not required.
  4. Check the end for defects. The weld end must be free of defects. Defects no deeper than 1.5 mm (1/16 in) are ground out under Clause 6.19.1. Anything deeper is excavated and repaired by welding under Clause 6.19.2.

D1.8 Figure 6.3 illustrates the finished condition. The point is not cosmetic. The end of a CJP flange weld sits at the flange tip, which strains heavily in a yielding beam. A rough gouge mark or a sharp step at that tip can start a crack that runs into the flange.

MT after a repaired tab site

Clause 7.8 adds one inspection rule. If the weld tab removal site is repaired by additional welding, magnetic particle testing (MT) is performed on the repaired area and the area immediately around it. Clause 7.9 requires MT by the yoke method under a written procedure that meets Annex G, which our article on ultrasonic and magnetic particle testing explains. A site finished by grinding alone does not trigger this rule, which is one more reason good shops aim to finish tab sites by grinding.

Where tabs come off and where they stay

D1.8 does not require all weld tabs to be removed. The Engineer shows on the contract documents where removal is needed, as Clause 1.4.1 requires. The commentary's Table C-1.1 summarizes frequently used practice:

Location Weld tabs
Moment frame, top flange to column flange Remove
Moment frame, bottom flange to column flange Remove
Continuity plates, end near the k-area Not recommended; stay if used
Continuity plates, end near the flange tips Remove
Concentrically braced frames, brace connections Stay
Eccentrically braced frames, link to column Remove
Eccentrically braced frames, brace to link Remove
Column splices Remove

The table is guidance; the project documents govern. It shows the logic, though: tabs come off where the weld end sits in a zone of high cyclic strain, and stay where the end is lightly stressed or where removal would do more harm than good.

Continuity plates: a special case

Continuity plates, the stiffener plates welded between column flanges in line with the beam flanges, have two ends against the column flange. One end is at the outboard edge, near the flange tips, where tabs can be used normally under Clause 6.16.1. The other is at the inboard corner, next to the column web-to-flange junction, the k-area.

Clause 6.16.4 says weld tabs must not be used at the inboard end unless the Engineer permits or requires them, and if they are used there, they are not removed unless the Engineer specifies removal. The commentary gives the reason: corner clips sized for the k-area leave little room for a tab, and removing a tab there by gouging or grinding is likely to cause more harm than leaving it. The weld ends at that corner may be cascaded or treated by other approaches, which both design and detailing need to plan for. The k-area itself is covered in our article on k-area, continuity plate and doubler welding.

End dams

An end dam is a small block, metallic or not, placed across the end of a weld joint to stop molten weld metal and slag from running out. Clause 6.17.1 allows either material. Clause 6.17.2 is the important part:

  • End dams must not be placed at either end of the weld joint itself.
  • End dams may be placed at the outboard ends of weld tabs, but only where the tabs will be removed when the weld is complete (Figure 6.4).

The commentary explains the reasoning. An end dam set directly at the end of the groove creates a corner, and weld metal placed into that corner is likely to contain defects, right at the edge of the real joint. An end dam at the far end of a tab moves that defect-prone corner onto the tab, which is later cut away. End dams do have real benefits: they stop molten metal and slag dripping from the joint, which reduces the risk of injury to workers below and the risk of fire. The commentary adds that the minimum tab length should still be kept when end dams are added to the tab ends.

Common weld tab problems

  • Tabs too short. A 10 mm tab on a 40 mm flange leaves starts and stops inside the real joint. The rule is the greater of 25 mm or the part thickness, up to 50 mm.
  • Tacks outside the joint. In a Protected Zone, a tab tacked to the face of the flange leaves a hard spot that must be ground out and repaired.
  • Gouging into the weld. An aggressive air carbon arc cut takes the tab and part of the weld end with it, creating an undersized corner.
  • Leaving it rough. A torch-cut tab stub with drag lines and a sharp step does not meet the 13 µm finish or the smooth contour requirement.
  • End dam on the joint. A dam placed at the end of a short groove, with no tab, traps defects at the flange tip.
  • Removing tabs at the continuity plate inboard corner. Unless the Engineer requires it, these stay.

Shop or field

Weld tabs belong to whoever makes the weld. On field-welded moment connections, which are common in the United States, the erector fits, welds and removes the tabs, and that is the US contractor's scope. On shop-welded column trees, continuity plates, built-up members and braced frame connections, it is shop work. Either way, the shop drawings should state for every joint type whether tabs are removed, whether end dams may be used and what finish is expected, so the welder on site and the inspector read the same requirement.

Questions a general contractor can ask

  1. Which joints require weld tab removal, and where is it shown on the shop drawings?
  2. What tab length is used for each flange thickness?
  3. How are tabs tacked inside Protected Zones?
  4. How is the finish of tab removal sites checked, and how are repairs recorded and tested?
  5. Are end dams used, and only on tabs that will be removed?

How World Steel handles weld tabs

World Steel shows the weld tab, end dam and finish requirement of every seismic joint type on the shop drawings, taken from the contract documents, and raises an RFI when a connection is unclear. On shop-welded joints, our welders size tabs to the Clause 6.16.1 rule, tack them inside the joint in Protected Zones, and remove and finish them where required, with the finish checked at our weld inspection and NDT checkpoint. Our shop welding procedures and welders are qualified to AWS D1.8, and tab removal and any repair MT are recorded in our IAS AC472-accredited quality system.

For the matching rules on steel backing, read our article on weld backing removal and reinforcing fillets.

Quick answers

How long must a weld tab be under AWS D1.8?

Where practicable, at least 25 mm (1 in) or the thickness of the part, whichever is greater, beyond the edge of the joint. It need not be longer than 50 mm (2 in).

How smooth must the edge be after weld tab removal?

No rougher than 13 µm (500 µin), judged with AWS C4.1 sample 4 as a guide. Grinding flush is not required, but the weld end must have a smooth contour with no notches or sharp corners.

Are weld tabs removed at continuity plates?

Not at the end next to the column web-to-flange junction. Tabs should not be used there unless the Engineer permits them, and if used they stay in place unless the Engineer says otherwise.

Where may end dams be placed?

Only at the outboard ends of weld tabs that will be removed after welding. End dams placed directly at the end of the weld joint are prohibited.

Keep building your steel plan

Go further on USPEB.com

Keep going in the series

AWS D1.8 seismic fabrication series

Twenty in-depth articles that follow a seismic weld from the drawings to the last test report. Each one explains a part of AWS D1.8:2025 in plain terms and lists the checks a general contractor can ask the fabricator about.

Drawings and scope

What the code covers, which welds are Demand Critical, and the data the drawings must carry.

Procedures and welders

The WPS, the restricted access welder test and the bottom flange sequence.

Details and Protected Zones

Access holes, backing, weld tabs, k-area details, Protected Zones and repairs.

Inspection and testing

Who inspects what, inspector qualifications, and UT and MT done the D1.8 way.

Bidding a large US project?

Send the bid documents, or just a footprint and an address. Our engineers check them against US code requirements and confirm what World Steel would supply, from a plant that fabricates 2,500 metric tons of structural steel a month.