Skip to content
Seeking US contractor partners IAS AC472 ACCREDITED ★ METAL BUILDINGS ★ AC472 IAS AC472 accreditedIAS AC472
World Steel USA

QC checkpoint: surface prep and coating

Paint goes on only when the steel and the air say yes

A coating fails at the surface underneath it long before it fails on its own. So the blast is accepted before primer goes on, the air and the steel are measured before every coat, and the thickness of each coat is read and written down per coating system, from the first coat to the last.

Before every coat

Go when

Steel temperature

At least 3 °C (5 °F) above the dew point, so no film of condensation is trapped under the coat.

Dew point

Worked out from air temperature and relative humidity before coating starts and again when conditions change.

Relative humidity

Within the limit on the coating manufacturer’s data sheet for that product.

Air and paint temperature

Never below 4 °C (39 °F), and within the range the data sheet allows.

Checked by the foreman and by QC. Outside the limits, coating stops.

Acceptance, coat by coat

Six gates between bare steel and a finished system

Each gate has a standard behind it, named in your specification or the coating manufacturer’s data. The blast is a hold point: no primer goes on until it is accepted.

  1. Before blasting

    Oil and grease removed; weld spatter, slag and sharp edges dressed so the coating can cover them.

    SSPC-SP 1 solvent cleaning

  2. Blast cleanliness

    Hold point

    The cleanliness grade your specification names, compared with reference photographs.

    AMPP/SSPC blast grades, such as SP 6 commercial or SP 10 near-white; SSPC-VIS 1

  3. Surface profile

    The anchor pattern deep enough for the primer to grip, checked against the data sheet range.

    ASTM D4417

  4. Each coat

    Dry film thickness read across the member and compared with the specified range for that coat.

    SSPC-PA 2, with gauges checked per ASTM D7091

  5. Adhesion

    Where the specification calls for it, the bond of the system is tested on the steel or on test panels.

    ASTM D3359 or ASTM D4541

  6. Galvanizing

    Where members are hot-dip galvanized instead, coating thickness and appearance are checked.

    ASTM A123

The record

One record per coat, per coating system

Written at the time, not afterward, and filed in the Manufacturing Data Record that ships with your steel. If a coating question comes up years later, the answer is on paper.

Roller conveyor carrying members into a shot-blasting machine
Coated members drying in rows on stands in the paint hall

Coating inspection record

  • Coating system and coat, with product name and color
  • Batch numbers and manufacture dates from the paint containers
  • Air temperature, steel temperature, humidity and dew point at the time
  • Blast grade accepted and surface profile readings
  • Dry film thickness readings and their average per member or area
  • Adhesion results where tested
  • Defects marked, repaired and closed, with photos
  • Inspector name and date

Measured by the people who mixed it

Paint checked at the can as well as on the steel

Each container is labeled with its batch number and manufacture date, mixed to the manufacturer’s instructions and thinned only with the thinner the data sheet allows. The batches used on each coat are written into your record, so a question about a product can be traced to the members it went on.

Verifying coating materials against the approved paint system
Verifying coating materials against the approved paint system. (IAS AC472 periodic audit, April 2022)

QC and QA

Who checks what at this checkpoint

US practice separates the fabricator’s quality control from the quality assurance carried out for the owner. World Steel runs the QC; your side decides how much QA it adds, and the Engineer of Record sets what is acceptable.

World Steel QC

Quality control: the fabricator

Checks conditions before every coat, accepts the blast before priming, measures each coat, marks and closes defects with photos, and records it all per coating system.

Your inspector

Quality assurance: owner, special or third-party inspector

Can hold the blast before priming as a hold point, witness thickness readings in the plant or by video, and review the coating records.

Your Engineer of Record

Sets the criteria, rules on what changes the design

Specifies the coating system, the blast grade, the thickness per coat and whether adhesion testing is required, usually with the coating manufacturer.

Inspectors can attend in Vietnam, join hold points live on Zoom or Microsoft Teams, or be given remote access to the records on request. The plant itself is audited twice a year under IAS AC472, with periodic plant inspections by Smith-Emery Laboratories.

Questions from US contractors and inspectors

Questions about surface preparation and coating checks

Ask us anything else about this checkpoint before you award, or during the job through your project manager.

Do you blast and paint indoors?

Yes. Blasting and painting are done indoors, and the foreman and QC check temperature and humidity before each coat and stop the work when conditions fall outside the limits.

What blast grade do you use?

The one your coating system and specification call for. Common grades are SSPC-SP 6 commercial blast and SSPC-SP 10 near-white blast. The grade is written into the ITP and accepted before primer goes on.

How is dry film thickness measured?

With calibrated gauges, following SSPC-PA 2, which sets how many readings are taken and how they are averaged across a member. Readings are taken for each coat, not only the total.

What happens when a coat is too thin or damaged?

QC marks the area on the member with a yellow paint marker and logs it on the punch list with a photo. It is repaired, measured again and closed with a photo before the member moves on.

Can you record the paint batches used on our job?

Yes. Each paint container is labeled with its batch number and manufacture date, and the batches used are written into the coating record for each coat.

Is the coating record included in our documents?

Yes. Conditions, blast acceptance, thickness readings and repairs for each coating system are part of the Manufacturing Data Record shipped with your steel.

Tell us how long your steel has to last

Send the exposure, the coating system or the specification section. We will plan the blast grade, the coats and the checks your inspector can hold before priming.